Hardness Conversion Chart (Rockwell C, Vickers, Brinell)

Approximate Rockwell C, Vickers and Brinell hardness equivalents for steel, with tensile strength estimates.

Hardness measures resistance to indentation. The scales you meet most are Rockwell C (HRC) for hardened steel, Vickers (HV) for any metal and thin sections, and Brinell (HB) for castings and forgings. For steel they can be converted approximately: HRC 40 is about HV 392 and HB 371; HRC 60, a hard tool steel, is about HV 697.

The table gives nine points from HRC 20 to 60 with the Vickers number, the Brinell number (to HRC 50) and the tensile strength estimated from it (tensile strength in MPa is about 3.45 × HB for carbon and low-alloy steels). The conversion is approximate and applies to non-austenitic steels.

The table

9 rows
Rockwell CVickers (HV)Brinell (HB, 3000 kgf)Approximate tensile strength (MPa)Approximate tensile strength (ksi)
HRC 20238226780113
HRC 25266253875127
HRC 30302286985143
HRC 353453271130164
HRC 403923711280186
HRC 454464211450211
HRC 505134811660241
HRC 55595–––
HRC 60697–––

Source and notes: Approximate conversion for non-austenitic steels after ASTM E140 (Standard Hardness Conversion Tables for Metals), rounded. Tensile strength is estimated as 3.45 times the Brinell number in MPa, which is accurate to roughly 10 percent for carbon and low-alloy steels and does not apply to austenitic stainless steel, cast iron or non-ferrous metals. Conversions between scales are approximate: measure in the scale that the specification asks for.

How to use this table

  1. Find the hardness you measured in the first (HRC) or second (HV) column and read across to the other scale.
  2. For intermediate values interpolate between rows; the relationship is smooth.
  3. Use the tensile strength column as a rough check only. For a design value use a tensile test or the supplier’s certificate.

Worked example: estimating the strength of a quenched and tempered shaft

  • A shaft measures HRC 30 on the Rockwell C scale: the table gives HV 302 and HB 286, so the tensile strength is about 3.45 × 286 = 987 MPa (143 ksi).
  • A part at HRC 45 has HV 446 and HB 421, and an estimated tensile strength of 1,452 MPa: about 47 percent stronger but also less ductile.

Notes and cautions

  • Conversions between hardness scales are empirical and not exact: different materials, heat treatments and indenter loads shift them. ASTM E140 gives tables for steel, nickel alloys, brass, aluminum and others.
  • Above about HRC 50 the Brinell scale is unreliable (the ball deforms) and is usually not quoted; this table leaves it out beyond HRC 50.
  • The tensile estimate does not apply to austenitic stainless steels, cast iron, aluminum or copper alloys, which need their own relations.
  • Case-hardened parts have a hard surface and a soft core: the surface hardness does not describe the core strength.

FAQ

What is HRC 40 in Brinell?

About HB 371 (and HV 392), with an estimated tensile strength of about 1,280 MPa.

How do you convert Rockwell C to Vickers?

Use the conversion table; for example HRC 50 is about HV 513 and HRC 60 about HV 697. The relation is approximate and applies to steel.

What is the relationship between hardness and tensile strength?

For carbon and low-alloy steels the tensile strength in MPa is approximately 3.45 times the Brinell hardness number.

Which hardness scale should I use?

HRC for hardened steel parts, HB for castings and soft metals, HV for thin sections, coatings and research. Use the scale the drawing or specification names.

Sources

  • ASTM E140, Standard Hardness Conversion Tables for Metals.
  • ASTM E18 (Rockwell), E92 (Vickers) and E10 (Brinell) test methods.
  • ASM Handbook, Volume 8: hardness testing.
  • Approximate conversion for non-austenitic steels after ASTM E140 (Standard Hardness Conversion Tables for Metals), rounded. Tensile strength is estimated as 3.45 times the Brinell number in MPa, which is accurate to roughly 10 percent for carbon and low-alloy steels and does not apply to austenitic stainless steel, cast iron or non-ferrous metals. Conversions between scales are approximate: measure in the scale that the specification asks for.

Published by Nick Peterson, mechanical engineer.