7075-T6 aluminum

Properties of 7075-T6 aluminum, each value tied to a recorded source.

A very high strength aerospace aluminum, much stronger than 6061-T6 in the published values. The sources describe weaker corrosion resistance and fair machinability, and it costs more than 6061, so it is used where strength matters most: gears, shafts, tooling plate and structural parts.

Family
Aluminum alloys
Condition
T6 and T651 (plate is supplied stress-relieved as T651); other tempers behave differently
Common forms
Plate, sheet, bar, extrusions
Alloy
7075 (Al-Zn-Mg-Cu)
Relative cost
$$$ Editorial, relative: noticeably more than 6061 aluminum, in the same range as stainless steel and below titanium. Not a quote; prices change.

Composition

Weight percent. The two sources agree on every limit.

ElementLimitsSource
Silicon (Si)0.40 max1,2
Iron (Fe)0.50 max1,2
Copper (Cu)1.20 to 2.001,2
Manganese (Mn)0.30 max1,2
Magnesium (Mg)2.10 to 2.901,2
Chromium (Cr)0.18 to 0.281,2
Zinc (Zn)5.10 to 6.101,2
Titanium (Ti)0.20 max1,2
Aluminum (Al)balance1,2

Properties

PropertySIUS customaryBasisSource
Physical
Density2.800 g/cm³0.101 lb/in³typical, nominal, 20 °C1
Density2.810 g/cm³0.102 lb/in³typical, temper not stated2
Mechanical
Elastic modulus (Young's)72.0 GPa10.4 Msitypical, temper not stated2
Yield strength476 MPa69.0 ksitypical, T6 sheet, 0.125 to 0.25 in thick (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.)1
Yield strength462 MPa67.0 ksitypical, T651 sheet, 0.25 to 0.50 in thick (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.)1
Yield strength469 MPa68.0 ksitypical, T651 sheet, 0.50 to 1.00 in thick (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.)1
Yield strength455 MPa66.0 ksitypical, T651 bar (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.)1
Tensile strength (ultimate or at break)538 MPa78.0 ksitypical, T6 sheet 0.125 to 0.25 in, and T651 sheet 0.25 to 1.00 in thick (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.)1
Tensile strength (ultimate or at break)531 MPa77.0 ksitypical, T651 bar (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.)1
Tensile strength (ultimate or at break)275 to 540 MPa39.9 to 78.3 ksirange, across all tempers (the sheet does not name one)2
Elongation at break8 %typical, T6 sheet, 0.125 to 0.25 in thick1
Elongation at break9 %typical, T651 sheet, 0.25 to 0.50 in thick1
Elongation at break7 %typical, T651 sheet 0.50 to 1.00 in thick, and T651 bar1
Thermal
Melting range, solidus532 °C990 °Ftypical, melting range1
Melting range, liquidus635 °C1,175 °Ftypical, melting range1
Melting point (as published)635 °C1,175 °Ftypical, published as a single melting point2
Thermal conductivity134 to 160 W/m·K929 to 1,109 BTU·in/h·ft²·°Frange, varies with temper2
Specific heat0.960 J/g·K0.229 BTU/lb·°Ftypical, 100 °C (Printed as 960 J/kg·K.)1

Specifications

  • AMS 4045: 7075-T6 sheet and T651 plate 1
  • AMS 4122: 7075-T6 cold finished rod, bar and wire 1
  • AMS 4123: 7075-T651 cold finished bar and rod 1
  • BS 2 L95: Alloy 7075-T651 plate 1
  • BS L170: Alloy 7075-T6511 bars and sections 1

What the sources say

  • Smiths Metal Centres describes 7075 as a very high strength aerospace aluminium for use where strength is critical and good corrosion resistance is not important, and rates its machinability as fair. 2
  • Aircraft Materials says the T173 and T7351 tempers have superior stress corrosion resistance and that the T6 and T651 tempers have fair machinability. 1

Things to know

  • Strength depends heavily on temper and thickness: the same stockist lists lower strength for the T7351 bar (68 ksi tensile) than for T651 bar (77 ksi), in exchange for better stress corrosion resistance.
  • Strength values here are labeled typical by the stockist and are not design minimums. Use the specification and your material certificate.

Sources

  1. Aircraft Materials (UK stockist): Aluminium Alloy 7075 Technical Data Sheet aircraftmaterials.com/data/aluminium/7075.html (distributor or reference site; read 2026-11-17)
  2. Smiths Metal Centres: 7075 Aluminium Technical Datasheet smithmetal.com/pdf/aluminium/7xxx/7075.pdf (distributor or reference site; read 2026-11-17)

Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.

All materials

Published by Nick Peterson, mechanical engineer.