5083 aluminum

Properties of 5083 aluminum, each value tied to a recorded source.

The strongest of the common non-heat-treatable aluminum alloys, known for seawater resistance and for keeping its strength after welding. It is used for ships, pressure vessels and truck bodies, but it should not be used where it stays warmer than about 65 °C.

Family
Aluminum alloys
Condition
O/H111 (annealed or lightly strain hardened); not heat treatable
Common forms
Plate, sheet and bar
Alloy
5083 (Al-Mg-Mn)
UNS
A95083
Relative cost
$$ Editorial, relative: a little above 5052 and 6061, plate is the usual form. Not a quote; prices change.

Composition

Weight percent. The two sources agree on every limit.

ElementLimitsSource
Silicon (Si)0.40 max2,1
Iron (Fe)0.40 max2,1
Copper (Cu)0.10 max2,1
Manganese (Mn)0.40 to 1.002,1
Magnesium (Mg)4.00 to 4.902,1
Chromium (Cr)0.05 to 0.252,1
Zinc (Zn)0.25 max2,1
Titanium (Ti)0.15 max2,1
Aluminum (Al)balance2,1

Properties

PropertySIUS customaryBasisSource
Physical
Density2.650 g/cm³0.0957 lb/in³typical, O/H1111
Mechanical
Elastic modulus (Young's)72.0 GPa10.4 Msitypical, O/H1111
Yield strength145 MPa21.0 ksitypical, proof stress, soft O/H1111
Yield strength110 MPa16.0 ksiminimum, temper O, extruded bar under 5 in diameter (16 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.)2
Yield strength166 MPa24.0 ksiminimum, temper H111, extruded bar under 5 in diameter (24 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.)2
Tensile strength (ultimate or at break)300 MPa43.5 ksitypical, soft O/H1111
Tensile strength (ultimate or at break)269 MPa39.0 ksiminimum, temper O, extruded bar under 5 in diameter (39 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.)2
Tensile strength (ultimate or at break)276 MPa40.0 ksiminimum, temper H111, extruded bar under 5 in diameter (40 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.)2
Elongation at break23 %typical, A50 mm, O/H1111
Elongation at break14 %minimum, in 2 in, temper O, extruded bar under 5 in diameter2
Elongation at break12 %minimum, in 2 in, temper H111, extruded bar under 5 in diameter2
Shear strength175 MPa25.4 ksitypical, O/H1111
Hardness, Vickers (HV)75 HVtypical, O/H1111
Thermal
Melting point (as published)570 °C1,058 °Ftypical, published as a single melting point1
Thermal conductivity121 W/m·K839 BTU·in/h·ft²·°Ftypical, O/H111; temperature not stated1
Thermal expansion (linear)25.0 µm/m·K13.9 µin/in·°Ftypical, O/H111; temperature range not stated1

Specifications

  • QQ-A-250/6: 5083 sheet and plate (listed as a similar specification) 2

What the sources say

  • Smiths Metal Centres describes 5083 as highly resistant to seawater and industrial chemical attack, with the highest strength of the non-heat-treatable alloys, retaining exceptional strength after welding, and not recommended above 65 °C. 1

Things to know

  • The two sources are on different bases: a typical set for the soft O/H111 condition and a table of minimums for extruded bar. None is a design value.

Sources

  1. Smiths Metal Centres: 5083 Aluminium Technical Datasheet smithmetal.com/pdf/aluminium/5xxx/5083.pdf (distributor or reference site; read 2026-11-17)
  2. Aircraft Materials (UK stockist): Aluminium Alloy 5083 Technical Data Sheet aircraftmaterials.com/data/aluminium/5083.html (distributor or reference site; read 2026-11-17)

Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.