Ti-6Al-4V (grade 5) titanium

Properties of Ti-6Al-4V (grade 5) titanium, each value tied to a recorded source.

The most widely used titanium alloy. It is about 60 percent as dense as steel with strength like a good alloy steel and excellent corrosion resistance, but it is expensive, hard to machine and weld, and loses strength above about 400 °C. It is used in aerospace, medical implants, racing and marine parts.

Family
Titanium alloys
Condition
Annealed or mill condition; heat treatable by solution treatment and aging in sections up to 25 mm (per Smiths)
Common forms
Bar, plate, sheet, wire, forgings and tube
Alloy
Ti-6Al-4V (alpha-beta)
UNS
R56400
ASTM
B348 Grade 5
AMS
4911, 4928
Relative cost
$$$ Editorial, relative: several times the cost of stainless steel and aluminum, and harder to machine. Not a quote; prices change.

Composition

Weight percent. Aircraft Materials prints its iron limit as 0.03, which looks like a typo (0.30 or 0.40); the Smiths value is used.

ElementLimitsSource
Aluminum (Al)5.50 to 6.752,1
Vanadium (V)3.50 to 4.502,1
Carbon (C)0.08 max2,1
Nitrogen (N)0.05 max2,1
Oxygen (O)0.20 max2,1
Hydrogen (H)0.02 max2,1
Iron (Fe)0.40 max1
Titanium (Ti)balance2,1

Properties

PropertySIUS customaryBasisSource
Physical
Density4.420 g/cm³0.160 lb/in³typical, printed as 4.42 kg/dm³1
Mechanical
Elastic modulus (Young's)114.0 GPa16.5 Msitypical, elastic modulus1
Yield strength828 MPa120 ksiminimum, 0.2 % proof stress, bar to ASTM B348 grade 51
Yield strength910 MPa132 ksitypical, 0.2 % proof stress, bar to ASTM B348 grade 51
Yield strength862 MPa125 ksiminimum, annealed bar under 2.00 in (125 ksi)2
Yield strength827 MPa120 ksiminimum, annealed bar 2.00 to 4.00 in and over 4.00 in (120 ksi)2
Tensile strength (ultimate or at break)895 MPa130 ksiminimum, bar to ASTM B348 grade 51
Tensile strength (ultimate or at break)1,000 MPa145 ksitypical, bar to ASTM B348 grade 51
Tensile strength (ultimate or at break)931 MPa135 ksiminimum, annealed bar under 2.00 in (135 ksi)2
Tensile strength (ultimate or at break)896 MPa130 ksiminimum, annealed bar 2.00 in and over (130 ksi)2
Elongation at break10 %minimum, in 4 diameters, bar to ASTM B348 grade 51
Elongation at break18 %typical, in 4 diameters, bar to ASTM B348 grade 51
Elongation at break10 %minimum, in 2 in, annealed bar up to 4 in; 8 % over 4 in2

Specifications

  • ASTM B348 Grade 5: titanium and titanium alloy bars and billets 1
  • AMS 4928: Ti-6Al-4V bar, wire, forgings and rings, annealed 2

What the sources say

  • Smiths Metal Centres calls grade 5 the most widely used high-strength titanium alloy, rates its weldability as fair, and says it can be used up to around 400 °C. 1

Things to know

  • The sources are on different bases: Smiths gives both a minimum and a typical value; Aircraft Materials gives annealed-bar minimums by diameter. Heat-treated and larger sections differ. None is a design value.
  • Grade 23 (ELI) has lower oxygen, better ductility and fracture toughness and somewhat lower strength; it is a different material.

Sources

  1. Smiths Metal Centres: Ti-6Al-4V (Grade 5) Technical Datasheet smithmetal.com/pdf/titanium/ti-6al-4v-grade-5.pdf (distributor or reference site; read 2026-11-17)
  2. Aircraft Materials (UK stockist): Titanium Alloy Grade 5 / Ti-6Al-4V Technical Data Sheet aircraftmaterials.com/data/titanium/ti6al4v.html (distributor or reference site; read 2026-11-17)

Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.

All materials

Published by Nick Peterson, mechanical engineer.