316 stainless steel (EN 1.4401)

Properties of 316 stainless steel (EN 1.4401), each value tied to a recorded source.

Stainless steel with molybdenum added for better resistance to chlorides and pitting than 304. It is the usual choice near salt water and in chemical and food processing, and it costs more than 304.

Family
Stainless steels: austenitic
Condition
Annealed (solution treated); data for bar and section up to 160 mm
Common forms
Sheet, strip, plate, bar, tube, pipe and fittings
EN
1.4401
Common name
316
Relative cost
$$$ Editorial, relative: above 304 stainless steel and 6061 aluminum, below titanium. Not a quote; prices change.

Composition

Weight percent per EN 10088-3:2005 as listed by the source.

ElementLimitsSource
Carbon (C)0.07 max1
Chromium (Cr)16.50 to 18.501,2
Molybdenum (Mo)2.00 to 2.501,2
Silicon (Si)1.00 max1,2
Phosphorus (P)0.05 max1,2
Sulfur (S)0.03 max1
Nickel (Ni)10.00 to 13.001,2
Manganese (Mn)2.00 max1,2
Nitrogen (N)0.11 max1
Iron (Fe)balance1,2

Properties

PropertySIUS customaryBasisSource
Physical
Density8.000 g/cm³0.289 lb/in³typical, typical for bar and section1
Density8.000 g/cm³0.289 lb/in³typical, printed as 8.00 kg/m³, a units slip for about 8000 kg/m³2
Mechanical
Elastic modulus (Young's)193.0 GPa28.0 Msitypical1
Elastic modulus (Young's)193.0 GPa28.0 Msitypical2
Yield strength200 MPa29.0 ksiminimum, proof stress, bar and section up to 160 mm1
Yield strength220 MPa31.9 ksiminimum, proof stress, minimum2
Tensile strength (ultimate or at break)500 to 700 MPa72.5 to 102 ksirange, bar and section up to 160 mm1
Tensile strength (ultimate or at break)520 to 680 MPa75.4 to 98.6 ksirange2
Elongation at break40 %minimum, A50 mm, bar and section up to 160 mm1
Elongation at break40 %minimum, A5, minimum2
Hardness, Brinell (HB)215 HBmaximum, Brinell, bar and section up to 160 mm1
Thermal
Melting point (as published)1,400 °C2,552 °Ftypical, published as a single melting point1
Melting point (as published)1,400 °C2,552 °Ftypical, published as a single melting point2
Thermal conductivity16 W/m·K113 BTU·in/h·ft²·°Ftypical, temperature not stated1
Thermal conductivity16 W/m·K113 BTU·in/h·ft²·°Ftypical, temperature not stated2
Thermal expansion (linear)15.9 µm/m·K8.83 µin/in·°Ftypical, temperature range not stated1
Thermal expansion (linear)15.9 µm/m·K8.83 µin/in·°Ftypical, temperature range not stated2
Electrical
Electrical resistivity740 nΩ·mtypical, printed as 0.74 x10^-6 ohm·m1

What the sources say

  • The source describes 316 as usually regarded as marine grade stainless steel but not resistant to warm sea water, with pitting and crevice corrosion possible in warm chloride environments and stress corrosion cracking above about 60 °C. 1

Things to know

  • Two distributor sources (Aalco, per EN 10088-3, and Smiths, a 316 and 316L sheet); both call their data indicative, so confirm against the standard and your material certificate.
  • The sources differ on minimum proof stress (200 and 220 MPa), the carbon limit (0.07 and 0.08 percent) and the sulfur limit; the range is shown. Smiths prints density as 8.00 kg/m³, a units slip for 8.00 g/cm³.

Sources

  1. Aalco Metals Limited: Stainless Steel, Austenitic, 1.4401 (316) Bar and Section (data per EN 10088-3:2005) aalco.co.uk/datasheets/Stainless-Steel-14401-316-Bar-and-Section_37.ashx (distributor or reference site; read 2026-11-17)
  2. Smiths Metal Centres: 316 / 316L Stainless Technical Datasheet smithmetal.com/pdf/stainless/316-316l-stainless.pdf (distributor or reference site; read 2026-11-17)

Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.

All materials