Copper C101 (CW004A)
Properties of Copper C101 (CW004A), each value tied to a recorded source.
Nearly pure copper: the best common conductor of heat and electricity and very easy to cold work and solder. It is soft, heavy and expensive, and used for busbars, heat sinks, wiring and electrical contacts rather than for structure.
Composition
Copper balance; others total 0.10 maximum per the source.
| Element | Limits | Source |
|---|---|---|
| Copper (Cu) | balance | 1,2 |
Properties
| Property | SI | US customary | Basis | Source |
|---|---|---|---|---|
| Physical | ||||
| Density | 8.920 g/cm³ | 0.322 lb/in³ | typical | 1 |
| Density | 8.920 g/cm³ | 0.322 lb/in³ | typical | 2 |
| Mechanical | ||||
| Elastic modulus (Young's) | 117.0 GPa | 17.0 Msi | typical | 1 |
| Elastic modulus (Young's) | 117.0 GPa | 17.0 Msi | typical | 2 |
| Yield strength | 50 to 340 MPa | 7.25 to 49.3 ksi | range, proof stress across tempers, sheet 0.2 to 15 mm | 1 |
| Yield strength | 50 to 340 MPa | 7.25 to 49.3 ksi | range, proof stress 0.2 % across tempers | 2 |
| Tensile strength (ultimate or at break) | 200 to 360 MPa | 29.0 to 52.2 ksi | range, across tempers, sheet 0.2 to 15 mm | 1 |
| Tensile strength (ultimate or at break) | 200 to 400 MPa | 29.0 to 58.0 ksi | range, across tempers | 2 |
| Elongation at break | 5 to 50 % | range, A50 mm across tempers (printed as 50 to 5) | 1 | |
| Elongation at break | 5 to 50 % | range, A5 across tempers | 2 | |
| Hardness, Vickers (HV) | 40 to 110 HV | range, across tempers | 1 | |
| Hardness, Vickers (HV) | 40 to 120 HV | range, VPN across tempers | 2 | |
| Thermal | ||||
| Melting point (as published) | 1,083 °C | 1,981 °F | typical, published as a single melting point | 1 |
| Melting point (as published) | 1,083 °C | 1,981 °F | typical, published as a single melting point | 2 |
| Thermal conductivity | 391 W/m·K | 2,712 BTU·in/h·ft²·°F | typical, temperature not stated | 1 |
| Thermal conductivity | 391 W/m·K | 2,712 BTU·in/h·ft²·°F | typical, temperature not stated | 2 |
| Thermal expansion (linear) | 16.9 µm/m·K | 9.39 µin/in·°F | typical, temperature range not stated | 1 |
| Thermal expansion (linear) | 16.9 µm/m·K | 9.39 µin/in·°F | typical, temperature range not stated | 2 |
| Electrical | ||||
| Electrical resistivity | 17 nΩ·m | typical, printed as 0.0171 x10^-6 ohm·m (100 % IACS) | 1 | |
| Electrical resistivity | 17 nΩ·m | typical, printed as 0.0171 x10^-6 ohm·m | 2 | |
What the sources say
- The source gives copper CW004A a machinability rating of 20, where brass CW614N is 100, and rates soldering as excellent, brazing and butt welding as good, and gas shielded arc welding as fair. 1
Things to know
- Two distributor sources (Aalco and Smiths) agree on every physical value. Strength depends strongly on temper (soft to hard), so each strength is shown as a range across tempers.
Sources
- Aalco Metals Limited: Copper and Copper Alloys, CW004A Sheet, Plate and Bar (data per EN 1652:1997 and EN 13601) aalco.co.uk/datasheets/Copper-and-Copper-Alloys-CW004A-Sheet-Plate-and-Bar_32.ashx (distributor or reference site; read 2026-11-17)
- Smiths Metal Centres: C101 Copper Technical Datasheet smithmetal.com/pdf/copper/c101.pdf (distributor or reference site; read 2026-11-17)
Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.