17-4 PH stainless steel (EN 1.4542)

Properties of 17-4 PH stainless steel (EN 1.4542), each value tied to a recorded source.

A precipitation hardening stainless steel with about 17 percent chromium, 4 percent nickel and 4 percent copper. It is machined in the solution annealed condition and then hardened by a single low-temperature aging treatment, which gives high strength with little distortion. Strength and hardness depend on the aging condition, from H900 (strongest) to H1150 (lowest strength, highest elongation).

Family
Stainless steels: precipitation hardening
Condition
Bar; supplied solution annealed (condition A) and aged to the H conditions (H900 to H1150) or the EN P conditions; every value states its condition
Common forms
Bar, forgings, plate, sheet and strip
EN
1.4542 (per Aalco and Aircraft Materials)
Common name
17-4 PH, grade 630
UNS
S17400
AISI
630 (per Smiths)
AMS
5643, 5622 (bar), 5604 (sheet and plate)
Relative cost
$$ Editorial, relative: above 304 stainless steel as bar (more alloy and an aging treatment), well below titanium. Not a quote; prices change.

Composition

Weight percent, AMS 5643 limits as printed by Smiths and Aircraft Materials. Aalco prints the EN 10088-3 limits for 1.4542, which differ for chromium (15.00 to 17.00), manganese (1.50), silicon (0.70) and molybdenum (0.60), so Aalco is cited only on the rows it agrees with. Niobium also has a minimum of 5 times the carbon content (Smiths; Aircraft Materials gives it for niobium plus tantalum). Aircraft Materials lists no molybdenum limit.

ElementLimitsSource
Carbon (C)0.07 max3,2,1
Chromium (Cr)15.00 to 17.503,2
Nickel (Ni)3.00 to 5.003,2,1
Copper (Cu)3.00 to 5.003,2,1
Manganese (Mn)1.00 max3,2
Silicon (Si)1.00 max3,2
Phosphorus (P)0.04 max3,2,1
Sulfur (S)0.03 max3,2,1
Niobium (Nb)0.45 max3,2,1
Molybdenum (Mo)0.50 max2
Iron (Fe)balance1

Properties

PropertySIUS customaryBasisSource
Physical
Density7.750 g/cm³0.280 lb/in³typical1
Density7.750 g/cm³0.280 lb/in³typical, printed as 7.75 kg/dm³2
Mechanical
Elastic modulus (Young's)196.0 GPa28.4 Msitypical1
Yield strength1,172 MPa170 ksitypical, H900, 0.2 % proof stress2
Yield strength1,069 MPa155 ksitypical, H925, 0.2 % proof stress2
Yield strength1,000 MPa145 ksitypical, H1025, 0.2 % proof stress2
Yield strength862 MPa125 ksitypical, H1075, 0.2 % proof stress2
Yield strength793 MPa115 ksitypical, H1100, 0.2 % proof stress2
Yield strength724 MPa105 ksitypical, H1150, 0.2 % proof stress2
Yield strength1,172 MPa170 ksitypical, H900, 0.2 % yield (170 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.)3
Yield strength1,069 MPa155 ksitypical, H925, 0.2 % yield (155 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.)3
Yield strength1,000 MPa145 ksitypical, H1025, 0.2 % yield (145 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.)3
Yield strength862 MPa125 ksitypical, H1075, 0.2 % yield (125 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.)3
Yield strength793 MPa115 ksitypical, H1100, 0.2 % yield (115 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.)3
Yield strength724 MPa105 ksitypical, H1150, 0.2 % yield (105 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.)3
Yield strength520 MPa75.4 ksiminimum, P800, proof stress, bar up to 100 mm1
Yield strength720 MPa104 ksiminimum, P930, proof stress, bar up to 100 mm1
Yield strength790 MPa115 ksiminimum, P960, proof stress, bar up to 100 mm1
Yield strength1,000 MPa145 ksiminimum, P1070, proof stress, bar up to 100 mm1
Tensile strength (ultimate or at break)1,310 MPa190 ksitypical, H9002
Tensile strength (ultimate or at break)1,172 MPa170 ksitypical, H9252
Tensile strength (ultimate or at break)1,069 MPa155 ksitypical, H10252
Tensile strength (ultimate or at break)1,000 MPa145 ksitypical, H10752
Tensile strength (ultimate or at break)965 MPa140 ksitypical, H11002
Tensile strength (ultimate or at break)931 MPa135 ksitypical, H11502
Tensile strength (ultimate or at break)1,310 MPa190 ksitypical, H900 (190 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.)3
Tensile strength (ultimate or at break)1,172 MPa170 ksitypical, H925 (170 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.)3
Tensile strength (ultimate or at break)1,069 MPa155 ksitypical, H1025 (155 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.)3
Tensile strength (ultimate or at break)1,000 MPa145 ksitypical, H1075 (145 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.)3
Tensile strength (ultimate or at break)965 MPa140 ksitypical, H1100 (140 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.)3
Tensile strength (ultimate or at break)931 MPa135 ksitypical, H1150 (135 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.)3
Tensile strength (ultimate or at break)1,200 MPa174 ksimaximum, solution annealed bar up to 100 mm1
Tensile strength (ultimate or at break)800 to 950 MPa116 to 138 ksirange, P800, bar up to 100 mm1
Tensile strength (ultimate or at break)930 to 1,100 MPa135 to 160 ksirange, P930, bar up to 100 mm1
Tensile strength (ultimate or at break)960 to 1,160 MPa139 to 168 ksirange, P960, bar up to 100 mm1
Tensile strength (ultimate or at break)1,070 to 1,270 MPa155 to 184 ksirange, P1070, bar up to 100 mm1
Elongation at break10 %typical, H900, on 4D gauge length2
Elongation at break10 %typical, H925, on 4D gauge length2
Elongation at break12 %typical, H1025, on 4D gauge length2
Elongation at break13 %typical, H1075, on 4D gauge length2
Elongation at break14 %typical, H1100, on 4D gauge length2
Elongation at break16 %typical, H1150, on 4D gauge length2
Elongation at break10 %typical, H900, in 2D3
Elongation at break10 %typical, H925, in 2D3
Elongation at break12 %typical, H1025, in 2D3
Elongation at break13 %typical, H1075, in 2D3
Elongation at break14 %typical, H1100, in 2D3
Elongation at break16 %typical, H1150, in 2D3
Elongation at break18 %minimum, P800, A, bar up to 100 mm1
Elongation at break16 %minimum, P930, A, bar up to 100 mm1
Elongation at break12 %minimum, P960, A, bar up to 100 mm1
Elongation at break10 %minimum, P1070, A, bar up to 100 mm1
Hardness, Brinell (HB)388 to 444 HBrange, H9002
Hardness, Brinell (HB)375 to 429 HBrange, H9252
Hardness, Brinell (HB)331 to 401 HBrange, H10252
Hardness, Brinell (HB)311 to 375 HBrange, H10752
Hardness, Brinell (HB)302 to 363 HBrange, H11002
Hardness, Brinell (HB)277 to 352 HBrange, H11502
Hardness, Brinell (HB)363 HBmaximum, condition A (solution annealed)3
Hardness, Brinell (HB)360 HBmaximum, solution annealed bar up to 100 mm1
Thermal
Thermal conductivity18 W/m·K128 BTU·in/h·ft²·°Ftypical, temperature not stated1
Thermal expansion (linear)10.8 µm/m·K6.00 µin/in·°Ftypical, temperature range not stated1
Electrical
Electrical resistivity800 nΩ·mtypical, printed as 0.8 x10^-6 ohm·m1

Specifications

  • AMS 5643: bars, wire, forgings, tubing and rings 3
  • AMS 5604: sheet, strip and plate 3
  • ASTM A564 Grade 630: listed as a specification (with ASME SA564) 3
  • ASME SA-564 Type 630: listed as a related specification 2
  • EN 10088-3:2005: composition and bar properties for 1.4542 (as cited by Aalco) 1

What the sources say

  • Smiths Metal Centres says the material should not be used in the annealed condition, that its corrosion resistance is superior to straight chromium grades like 410 and approaches the chromium-nickel grades, and that it is readily weldable without the pre-heat and post-heat used for other hardenable stainless grades. 2
  • Aalco says the corrosion resistance is similar to grade 304, that 17-4 PH is susceptible to pitting and crevice corrosion in warm chloride environments, and that parts shrink slightly when aged: about 0.05 percent for H900 and 0.10 percent for H1150. 1
  • Aalco advises against prolonged exposure to 370 to 480 °C where toughness at room temperature matters, and against use above the precipitation hardening temperature. 1

Things to know

  • Three distributor sources; all disclaim their data (indicative, approximate or guideline only), so confirm against the specification and your material certificate. Strength depends on the aging condition: H900 is the strongest and H1150 the most ductile.
  • Smiths and Aircraft Materials both label their H-condition values as typical and agree once the ksi values are converted. Aalco gives EN 10088-3 minimums and ranges for the P800 to P1070 conditions, which are different heat treatments from the H conditions, so they are listed separately.
  • The Aircraft Materials bar table heads its hardness column "Rockwell C" but prints Brinell-like numbers (388-444 and so on), so its H-condition hardness is not used; Smiths gives the same ranges as Brinell. Aircraft Materials also gives sheet hardness in Rockwell C, which this library has no field for.
  • Aalco's Heat Treatment section shows a QT 650 to QT 900 tensile list that does not match this grade's conditions, so it is not used.

Sources

  1. Aalco Metals Limited: Stainless Steel, Precipitation Hardening, 1.4542 (17/4 and 630) Bar (data per EN 10088-3:2005) aalco.co.uk/datasheets/Stainless-Steel-14542-174--630-Bar_100.ashx (distributor or reference site; read 2026-11-17)
  2. Smiths Metal Centres: AMS 5643 (17/4 PH) Precipitation Hardening Stainless Steel Bar Technical Datasheet smithmetal.com/pdf/stainless/ph/17-4ph.pdf (distributor or reference site; read 2026-11-17)
  3. Aircraft Materials (UK stockist): Stainless Steel 17-4PH Bar (AMS 5643 / AMS 5622) Technical Data Sheet aircraftmaterials.com/data/alstst/ams5643.html (distributor or reference site; read 2026-11-17)

Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.