2024 aluminum
Properties of 2024 aluminum, each value tied to a recorded source.
A high-strength aluminum-copper alloy, used mainly for aircraft structure because of its good fatigue resistance. Its resistance to atmospheric corrosion is poor, so parts are usually protected and sheet is also sold clad with a pure aluminum layer.
Composition
Weight percent. Aircraft Materials (its "Alloy 2024 USA" row), Smiths and Kaiser agree on every limit shown. Aircraft Materials also prints a different French 2024A row, which is not used. Gabrian prints manganese as 0.5 to 0.6, which does not match the others, so its composition is not used. Other elements: 0.05 each (all three) and 0.15 total (Aircraft Materials and Kaiser).
| Element | Limits | Source |
|---|---|---|
| Silicon (Si) | 0.50 max | 4,1,3 |
| Iron (Fe) | 0.50 max | 4,1,3 |
| Copper (Cu) | 3.80 to 4.90 | 4,1,3 |
| Manganese (Mn) | 0.30 to 0.90 | 4,1,3 |
| Magnesium (Mg) | 1.20 to 1.80 | 4,1,3 |
| Chromium (Cr) | 0.10 max | 4,1,3 |
| Zinc (Zn) | 0.25 max | 4,1,3 |
| Titanium (Ti) | 0.15 max | 4,1,3 |
| Aluminum (Al) | balance | 4,1,3 |
Properties
| Property | SI | US customary | Basis | Source |
|---|---|---|---|---|
| Physical | ||||
| Density | 2.770 g/cm³ | 0.100 lb/in³ | typical, nominal, 20 °C (Printed as 2.77 Mg/m³.) | 1 |
| Density | 2.780 g/cm³ | 0.100 lb/in³ | typical, T3, T4/T351 and T851 columns | 2 |
| Mechanical | ||||
| Elastic modulus (Young's) | 73.1 GPa | 10.6 Msi | typical, all tempers listed (O, T4/T351, T361, T851, T861) | 1 |
| Elastic modulus (Young's) | 73.1 GPa | 10.6 Msi | typical, T3 and T4/T351 columns (basis not printed) | 2 |
| Elastic modulus (Young's) | 72.4 GPa | 10.5 Msi | typical, T851 column (basis not printed) | 2 |
| Yield strength | 76 MPa | 11.0 ksi | typical, O | 1 |
| Yield strength | 324 MPa | 47.0 ksi | typical, T4 and T351 | 1 |
| Yield strength | 393 MPa | 57.0 ksi | typical, T361 | 1 |
| Yield strength | 414 MPa | 60.0 ksi | typical, T851 | 1 |
| Yield strength | 455 MPa | 66.0 ksi | typical, T861 | 1 |
| Yield strength | 96 MPa | 13.9 ksi | maximum, O sheet and plate, 0.25 to 12.44 mm (printed as max) | 3 |
| Yield strength | 289 MPa | 41.9 ksi | minimum, T3 flat sheet, 0.203 to 6.32 mm; basis not printed on the sheet, recorded as a minimum | 3 |
| Yield strength | 282 to 289 MPa | 40.9 to 41.9 ksi | range, T351 plate, 6.35 to 101.60 mm; basis not printed on the sheet, recorded as a minimum | 3 |
| Yield strength | 276 MPa | 40.0 ksi | minimum, T4 coiled sheet, 0.254 to 3.16 mm; basis not printed on the sheet, recorded as a minimum | 3 |
| Yield strength | 400 MPa | 58.0 ksi | minimum, T81 flat sheet, 0.254 to 6.32 mm; basis not printed on the sheet, recorded as a minimum | 3 |
| Yield strength | 393 to 400 MPa | 57.0 to 58.0 ksi | range, T851 plate, 6.35 to 38.07 mm; basis not printed on the sheet, recorded as a minimum | 3 |
| Yield strength | 345 MPa | 50.0 ksi | typical, T3 column (basis not printed) | 2 |
| Yield strength | 324 MPa | 47.0 ksi | typical, column headed "2024-4, -T351" as printed (basis not printed) | 2 |
| Yield strength | 400 MPa | 58.0 ksi | minimum, T851 column, printed as >= 400 MPa | 2 |
| Tensile strength (ultimate or at break) | 186 MPa | 27.0 ksi | typical, O, 0.500 in diameter specimen | 1 |
| Tensile strength (ultimate or at break) | 469 MPa | 68.0 ksi | typical, T4 and T351 | 1 |
| Tensile strength (ultimate or at break) | 496 MPa | 71.9 ksi | typical, T361 | 1 |
| Tensile strength (ultimate or at break) | 448 MPa | 65.0 ksi | typical, T851 | 1 |
| Tensile strength (ultimate or at break) | 483 MPa | 70.1 ksi | typical, T861 | 1 |
| Tensile strength (ultimate or at break) | 220 MPa | 31.9 ksi | maximum, O sheet and plate, 0.25 to 12.44 mm (printed as max) | 3 |
| Tensile strength (ultimate or at break) | 434 to 441 MPa | 62.9 to 64.0 ksi | range, T3 flat sheet, 0.203 to 6.32 mm; basis not printed on the sheet, recorded as a minimum | 3 |
| Tensile strength (ultimate or at break) | 393 to 441 MPa | 57.0 to 64.0 ksi | range, T351 plate, 6.35 to 101.60 mm, falling as thickness rises; basis not printed on the sheet, recorded as a minimum | 3 |
| Tensile strength (ultimate or at break) | 427 MPa | 61.9 ksi | minimum, T4 coiled sheet, 0.254 to 3.16 mm; basis not printed on the sheet, recorded as a minimum | 3 |
| Tensile strength (ultimate or at break) | 462 MPa | 67.0 ksi | minimum, T81 flat sheet, 0.254 to 6.32 mm; basis not printed on the sheet, recorded as a minimum | 3 |
| Tensile strength (ultimate or at break) | 455 to 462 MPa | 66.0 to 67.0 ksi | range, T851 plate, 6.35 to 38.07 mm; basis not printed on the sheet, recorded as a minimum | 3 |
| Tensile strength (ultimate or at break) | 483 MPa | 70.1 ksi | typical, T3 column (basis not printed) | 2 |
| Tensile strength (ultimate or at break) | 469 MPa | 68.0 ksi | typical, column headed "2024-4, -T351" as printed (basis not printed) | 2 |
| Tensile strength (ultimate or at break) | 455 MPa | 66.0 ksi | minimum, T851 column, printed as >= 455 MPa | 2 |
| Elongation at break | 22 % | typical, O, in 4D | 1 | |
| Elongation at break | 19 % | typical, T4 and T351, in 4D | 1 | |
| Elongation at break | 13 % | typical, T361, in 4D | 1 | |
| Elongation at break | 6 % | typical, T851 and T861, in 4D | 1 | |
| Elongation at break | 12 % | minimum, O sheet and plate; basis not printed on the sheet, recorded as a minimum | 3 | |
| Elongation at break | 10 to 15 % | range, T3 flat sheet, 0.203 to 6.32 mm; basis not printed on the sheet, recorded as a minimum | 3 | |
| Elongation at break | 4 to 12 % | range, T351 plate, 6.35 to 101.60 mm; basis not printed on the sheet, recorded as a minimum | 3 | |
| Elongation at break | 12 to 15 % | range, T4 coiled sheet, 0.254 to 3.16 mm; basis not printed on the sheet, recorded as a minimum | 3 | |
| Elongation at break | 5 % | minimum, T81 flat sheet and T851 plate; basis not printed on the sheet, recorded as a minimum | 3 | |
| Hardness, Brinell (HB) | 47 HB | typical, Brinell, 500 kg, 10 mm ball, O | 1 | |
| Hardness, Brinell (HB) | 120 HB | typical, Brinell, T4 and T351 | 1 | |
| Hardness, Brinell (HB) | 130 HB | typical, Brinell, T361 | 1 | |
| Shear strength | 124 MPa | 18.0 ksi | typical, O | 1 |
| Shear strength | 283 MPa | 41.0 ksi | typical, T4 and T351 | 1 |
| Shear strength | 290 MPa | 42.1 ksi | typical, T361 and T861 | 1 |
| Shear strength | 276 MPa | 40.0 ksi | typical, T851 | 1 |
| Fatigue strength | 90 MPa | 13.1 ksi | typical, O, R.R. Moore, 5 x 10^8 cycles of reversed stress | 1 |
| Fatigue strength | 138 MPa | 20.0 ksi | typical, T4 and T351, R.R. Moore, 5 x 10^8 cycles | 1 |
| Fatigue strength | 124 MPa | 18.0 ksi | typical, T361, R.R. Moore, 5 x 10^8 cycles | 1 |
| Thermal | ||||
| Melting range, solidus | 502 °C | 936 °F | typical, bottom of the printed melting range | 1 |
| Melting range, liquidus | 638 °C | 1,180 °F | typical, top of the printed melting range | 1 |
| Thermal conductivity | 190 W/m·K | 1,317 BTU·in/h·ft²·°F | typical, O temper, 20 °C | 1 |
| Thermal conductivity | 120 W/m·K | 832 BTU·in/h·ft²·°F | typical, T4, T351 and T451, 20 °C | 1 |
| Thermal conductivity | 121 W/m·K | 839 BTU·in/h·ft²·°F | typical, T3 and T4/T351 columns | 2 |
| Thermal conductivity | 151 W/m·K | 1,047 BTU·in/h·ft²·°F | typical, T851 column | 2 |
| Specific heat | 0.875 J/g·K | 0.209 BTU/lb·°F | typical, at 100 °C (Printed as 875 J/(kg·K).) | 1 |
| Thermal expansion (linear) | 22.9 µm/m·K | 12.7 µin/in·°F | typical, linear, 20 to 100 °C | 1 |
| Thermal expansion (linear) | 23.2 µm/m·K | 12.9 µin/in·°F | typical, linear, 20 to 100 °C, all three columns | 2 |
Specifications
- QQ-A-250/4: 2024 sheet and plate, O, T351, T851 (listed by the stockist) 4
- AMS 4037: 2024 sheet T3, plate T351 (listed by the stockist) 4
- BS L97: 2024 plate T351 (listed by the stockist) 4
What the sources say
- Smiths Metal Centres describes 2024 as having good fatigue resistance, especially in thick plate, and poor resistance to atmospheric attack, and says it is specified for fuselage structures and wing tension members. 3
- Kaiser Aluminum says 2024 has good machining characteristics and is popular for cold heading and thread rolling, with only fair corrosion resistance and anodizability. 1
Things to know
- The sources are on different bases. Kaiser prints typical values. Smiths prints values by temper and thickness without saying whether they are typical or minimum; they are recorded here as minimums because the same publisher's Smiths High Performance sheet prints the matching rows as minimums. Gabrian prints no basis except ">=" on its T851 strengths. None is a design value.
- Physical properties come from Kaiser and Gabrian only (Smiths prints none). Specific heat and the melting range come from Kaiser alone. Kaiser also prints conductivity rows for a "T651" temper that its mechanical table does not list; they are left out.
- Strength falls as plate gets thicker. Order to the specification and temper on the drawing and use the mill certificate.
Sources
- Kaiser Aluminum: Sheet Coil & Plate Alloy 2024 Technical Data (Rev. 05/06): typical mechanical properties by temper, composition limits, typical physical properties protolabs.com/media/bc1ilo5e/2024_t351-cnc.pdf (the maker of the material; read 2026-11-17)
- Gabrian International (aluminum extruder): 2024 Aluminum Alloy: Properties (T3, T4/T351 and T851 columns) gabrian.com/wp-content/uploads/2018/10/2024-Aluminum-Alloy-Properties.pdf (distributor or reference site; read 2026-11-17)
- Smiths Metal Centres: 2024 Aluminium Technical Datasheet (high strength aluminium alloy) smithmetal.com/pdf/aluminium/2xxx/2024.pdf (distributor or reference site; read 2026-11-17)
- Aircraft Materials (UK stockist): Aluminium Alloy 2024 Technical Data Sheet aircraftmaterials.com/data/aluminium/2024.html (distributor or reference site; read 2026-11-17)
Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.