Galvanic Corrosion Chart (Anodic Index and Compatible Metals)

The anodic index of metals and finishes (MIL-STD-889) and the rule for choosing compatible metal pairs.

Galvanic corrosion happens when two different metals touch in the presence of an electrolyte (water, salt, humidity): the more active metal (the anode) corrodes faster and the nobler metal (the cathode) is protected. The anodic index measures how active a metal is: the larger the difference between two metals, the worse the corrosion of the more anodic one.

The table lists 19 groups of metals and finishes from gold (0.00 V, most noble) to magnesium (1.75 V, most active), in the order of MIL-STD-889. A common design rule is to keep the difference below about 0.25 V indoors and about 0.15 V outdoors or in marine service.

The table

19 rows
Metal or finishAnodic index (V)End of the series
Gold, solid or plated; platinum0.00Cathodic (noble)
Rhodium plating0.05
Silver, solid or plated0.15
Nickel, solid or plated; titanium alloys; Monel0.30
Copper, solid or plated; low brasses and bronzes; silver solder0.35
Brass and bronzes0.40
High brasses and bronzes0.45
Stainless steel, 18 percent chromium type (passive)0.50
Chromium plate; tin plate; 12 percent chromium stainless0.60
Tin-lead solder0.65
Lead; lead-tin solders0.70
Aluminum, wrought 2000 series0.75
Iron, wrought, gray or malleable; plain carbon and low-alloy steel0.85
Aluminum, wrought alloys other than 2000 series; cast silicon-type aluminum0.90
Aluminum, other cast alloys; cadmium plate0.95
Hot-dip zinc plate; galvanized steel1.20
Zinc, wrought; zinc die casting; zinc plate1.25
Magnesium and magnesium alloys1.75Anodic (active)
Beryllium1.85

Source and notes: Anodic index values from MIL-STD-889 (Dissimilar Metals), measured in seawater against gold. The potential difference between two metals is the difference of their anodic indices; the metal with the larger index is the anode and corrodes. A common rule is to keep the difference below 0.25 V in a benign indoor environment and below about 0.15 V outdoors or in marine service.

How to use this table

  1. Look up the anodic index of each of the two metals and subtract. The metal with the larger value is the one that will corrode.
  2. Under about 0.15 V the pair is generally compatible even outdoors; above 0.25 V, isolate the metals, plate them, or choose a different pair.
  3. The area ratio matters: a small anode on a large cathode corrodes fast, while a large anode with a small cathode (a steel fastener in a large aluminum panel) corrodes slowly.

Worked example: stainless steel bolts in an aluminum bracket

  • Aluminum has an anodic index of 0.90 V and 18 percent chromium stainless steel 0.50 V. The difference is 0.40 V: the aluminum is the anode and will corrode where the two meet in a wet or salty place.
  • Plain carbon steel against the same stainless steel differs by 0.35 V, which is also too much for outdoor use without protection.
  • Fixes: insulate with a plastic washer or sleeve, plate the stainless, apply sealant or paint to keep the electrolyte out, or choose a closer pair such as anodized aluminum with 304 stainless fasteners coated with zinc-rich paste.

Notes and cautions

  • The anodic index is a screening tool. Real corrosion rates depend on the electrolyte, temperature, oxygen, the surface films, and the area ratio of the two metals.
  • Passive films matter: stainless steel is nobler when its oxide film is intact and active when it is not (in crevices or low-oxygen water).
  • Dry indoor environments with no condensation allow almost any combination; the risk is in wet, humid, marine and chemical-processing environments.
  • Prevention in order of effectiveness: choose compatible metals, keep the electrolyte out (sealant, coatings), insulate the metals from each other, plate or coat the cathode (never only the anode).

FAQ

What is galvanic corrosion?

Corrosion that occurs when two dissimilar metals are in electrical contact in a conductive liquid: the more active metal corrodes and the nobler one is protected.

What is the anodic index?

The potential in volts of a metal against gold in seawater (MIL-STD-889). A lower number means a nobler metal; the difference between two metals tells how strong the galvanic effect is.

Can I use stainless steel screws in aluminum?

Yes with care: the pair is 0.4 V apart, so outdoors use an insulating washer or sealant. The small stainless screw (cathode) in a large aluminum panel (anode) usually corrodes the aluminum only slowly.

Which metals are compatible with aluminum?

Zinc, cadmium plating and other aluminum alloys (within 0.15 V). Copper, brass and stainless steel need isolation in wet conditions.

Sources

  • MIL-STD-889, Dissimilar Metals.
  • ASM Handbook, Volume 13: Corrosion.
  • Davis, J. R. (ed.), Corrosion: Understanding the Basics, ASM International.
  • Anodic index values from MIL-STD-889 (Dissimilar Metals), measured in seawater against gold. The potential difference between two metals is the difference of their anodic indices; the metal with the larger index is the anode and corrodes. A common rule is to keep the difference below 0.25 V in a benign indoor environment and below about 0.15 V outdoors or in marine service.

Published by Nick Peterson, mechanical engineer.