2011 aluminum
Properties of 2011 aluminum, each value tied to a recorded source.
The free-machining aluminum: lead and bismuth make it break into small chips, so it is the choice for screw-machine parts, fittings and fasteners cut on automatic lathes. It is strong for an aluminum, but it has poor corrosion resistance and weldability and normally needs anodizing for protection.
Composition
Weight percent. The two sources agree on every limit.
| Element | Limits | Source |
|---|---|---|
| Silicon (Si) | 0.40 max | 2,1 |
| Iron (Fe) | 0.70 max | 2,1 |
| Copper (Cu) | 5.00 to 6.00 | 2,1 |
| Zinc (Zn) | 0.30 max | 2,1 |
| Lead (Pb) | 0.20 to 0.60 | 2,1 |
| Bismuth (Bi) | 0.20 to 0.60 | 2,1 |
| Aluminum (Al) | balance | 2,1 |
Properties
| Property | SI | US customary | Basis | Source |
|---|---|---|---|---|
| Physical | ||||
| Density | 2.820 g/cm³ | 0.102 lb/in³ | typical (Printed as 2.82 kg/m³, a units slip for g/cm³.) | 1 |
| Mechanical | ||||
| Elastic modulus (Young's) | 71.0 GPa | 10.3 Msi | typical | 1 |
| Yield strength | 290 MPa | 42.1 ksi | typical, proof stress, T3 | 1 |
| Yield strength | 270 MPa | 39.2 ksi | typical, proof stress, T4 | 1 |
| Yield strength | 300 MPa | 43.5 ksi | typical, proof stress, T6 | 1 |
| Yield strength | 315 MPa | 45.7 ksi | typical, proof stress, T8 | 1 |
| Yield strength | 255 MPa | 37.0 ksi | minimum, bar, temper TD (as printed), under 35 mm | 2 |
| Yield strength | 230 MPa | 33.4 ksi | minimum, bar, temper TD, 35 to 50 mm | 2 |
| Yield strength | 225 MPa | 32.6 ksi | minimum, bar, temper TF (as printed), under 65 mm | 2 |
| Yield strength | 195 MPa | 28.3 ksi | minimum, bar, temper TF, over 65 mm | 2 |
| Tensile strength (ultimate or at break) | 365 MPa | 52.9 ksi | typical, T3 | 1 |
| Tensile strength (ultimate or at break) | 350 MPa | 50.8 ksi | typical, T4 | 1 |
| Tensile strength (ultimate or at break) | 395 MPa | 57.3 ksi | typical, T6 | 1 |
| Tensile strength (ultimate or at break) | 420 MPa | 60.9 ksi | typical, T8 | 1 |
| Tensile strength (ultimate or at break) | 310 MPa | 45.0 ksi | minimum, bar, temper TD (as printed), under 35 mm | 2 |
| Tensile strength (ultimate or at break) | 295 MPa | 42.8 ksi | minimum, bar, temper TD, 35 to 50 mm | 2 |
| Tensile strength (ultimate or at break) | 310 MPa | 45.0 ksi | minimum, bar, temper TF (as printed), under 65 mm | 2 |
| Tensile strength (ultimate or at break) | 295 MPa | 42.8 ksi | minimum, bar, temper TF, over 65 mm | 2 |
| Elongation at break | 15 % | typical, A5, T3 | 1 | |
| Elongation at break | 18 % | typical, A5, T4 | 1 | |
| Elongation at break | 12 % | typical, A5, T6 | 1 | |
| Elongation at break | 13 % | typical, A5, T8 | 1 | |
| Elongation at break | 6 % | minimum, on 50 mm, bar TD under 10 mm | 2 | |
| Elongation at break | 8 % | minimum, on 50 mm, bar TD or TF over 10 mm | 2 | |
| Hardness, Brinell (HB) | 95 HB | typical, Brinell, T3 | 1 | |
| Hardness, Brinell (HB) | 90 HB | typical, Brinell, T4 | 1 | |
| Hardness, Brinell (HB) | 110 HB | typical, Brinell, T6 | 1 | |
| Hardness, Brinell (HB) | 115 HB | typical, Brinell, T8 | 1 | |
| Shear strength | 220 MPa | 31.9 ksi | typical, T3 | 1 |
| Shear strength | 210 MPa | 30.5 ksi | typical, T4 | 1 |
| Shear strength | 235 MPa | 34.1 ksi | typical, T6 | 1 |
| Shear strength | 250 MPa | 36.3 ksi | typical, T8 | 1 |
| Fatigue strength | 250 MPa | 36.3 ksi | typical, endurance limit, all tempers listed | 1 |
| Thermal | ||||
| Melting point (as published) | 535 °C | 995 °F | typical, published as a single melting point | 1 |
| Thermal conductivity | 138 W/m·K | 957 BTU·in/h·ft²·°F | typical, temperature not stated | 1 |
| Thermal expansion (linear) | 23.0 µm/m·K | 12.8 µin/in·°F | typical, temperature range not stated | 1 |
Specifications
- QQ-A-225/3: 2011 bar (listed as a similar specification) 2
What the sources say
- Smiths Metal Centres calls 2011 a free-machining alloy with excellent machinability and poor corrosion resistance and weldability, usually anodized, and suited to automatic lathes. 1
Things to know
- The two sources are on different bases: Smiths gives typical values by temper, Aircraft Materials gives bar minimums under its own temper codes (TD and TF), which are not mapped to T3 and T6 here.
- Contains lead and bismuth: check the rules for your product (for example drinking-water and RoHS limits).
Sources
- Smiths Metal Centres: 2011 Aluminium Technical Datasheet (free machining alloy) smithmetal.com/pdf/aluminium/2xxx/2011.pdf (distributor or reference site; read 2026-11-17)
- Aircraft Materials (UK stockist): Aluminium Alloy 2011 Technical Data Sheet aircraftmaterials.com/data/aluminium/2011.html (distributor or reference site; read 2026-11-17)
Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.