3003 aluminum
Properties of 3003 aluminum, each value tied to a recorded source.
The everyday low-cost sheet aluminum: about 20 percent stronger than pure 1100, very formable, welds well and resists corrosion. It is used for cookware, ducts, tanks, roofing and general sheet-metal work, but it is much weaker than 5052 or 6061.
Composition
Weight percent. Manganese comes from Aircraft Materials (1.0 to 1.5); Smiths prints a lower limit of 1.10, so it is not used for that row. Magnesium appears only on the Smiths sheet.
| Element | Limits | Source |
|---|---|---|
| Silicon (Si) | 0.60 max | 2,1 |
| Iron (Fe) | 0.70 max | 2,1 |
| Copper (Cu) | 0.05 to 0.20 | 2,1 |
| Zinc (Zn) | 0.10 max | 2,1 |
| Manganese (Mn) | 1.00 to 1.50 | 2 |
| Magnesium (Mg) | 0.05 max | 1 |
| Aluminum (Al) | balance | 2,1 |
Properties
| Property | SI | US customary | Basis | Source |
|---|---|---|---|---|
| Physical | ||||
| Density | 2.730 g/cm³ | 0.0986 lb/in³ | typical, O | 1 |
| Mechanical | ||||
| Elastic modulus (Young's) | 69.5 GPa | 10.1 Msi | typical, O | 1 |
| Yield strength | 50 MPa | 7.25 ksi | typical, proof stress, soft O condition | 1 |
| Yield strength | 35 MPa | 5.00 ksi | minimum, O, 0.064 in sheet (5 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 2 |
| Yield strength | 83 MPa | 12.0 ksi | minimum, H12, 0.064 in sheet (12 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 2 |
| Yield strength | 117 MPa | 17.0 ksi | minimum, H14, 0.064 in sheet (17 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 2 |
| Yield strength | 145 MPa | 21.0 ksi | minimum, H16, 0.064 in sheet (21 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 2 |
| Yield strength | 166 MPa | 24.0 ksi | minimum, H18, 0.064 in sheet (24 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 2 |
| Tensile strength (ultimate or at break) | 110 MPa | 16.0 ksi | typical, soft O condition | 1 |
| Tensile strength (ultimate or at break) | 97 to 131 MPa | 14.0 to 19.0 ksi | range, O, 0.064 in sheet (14 to 19 ksi as printed) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 2 |
| Tensile strength (ultimate or at break) | 117 to 159 MPa | 17.0 to 23.0 ksi | range, H12, 0.064 in sheet (17 to 23 ksi as printed) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 2 |
| Tensile strength (ultimate or at break) | 138 to 179 MPa | 20.0 to 26.0 ksi | range, H14, 0.064 in sheet (20 to 26 ksi as printed) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 2 |
| Tensile strength (ultimate or at break) | 166 to 207 MPa | 24.0 to 30.0 ksi | range, H16, 0.064 in sheet (24 to 30 ksi as printed) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 2 |
| Tensile strength (ultimate or at break) | 186 MPa | 27.0 ksi | minimum, H18, 0.064 in sheet (27 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 2 |
| Elongation at break | 25 % | typical, A50 mm, O | 1 | |
| Elongation at break | 25 % | minimum, in 2 in, O, 0.064 in sheet | 2 | |
| Elongation at break | 6 % | minimum, in 2 in, H12, 0.064 in sheet | 2 | |
| Elongation at break | 5 % | minimum, in 2 in, H14, 0.064 in sheet | 2 | |
| Elongation at break | 4 % | minimum, in 2 in, H16 and H18, 0.064 in sheet | 2 | |
| Shear strength | 75 MPa | 10.9 ksi | typical, O | 1 |
| Hardness, Vickers (HV) | 29 HV | typical, O | 1 | |
| Thermal | ||||
| Melting point (as published) | 655 °C | 1,211 °F | typical, published as a single melting point | 1 |
| Thermal conductivity | 190 W/m·K | 1,317 BTU·in/h·ft²·°F | typical, O; temperature not stated | 1 |
| Thermal expansion (linear) | 23.1 µm/m·K | 12.8 µin/in·°F | typical, O; temperature range not stated | 1 |
Specifications
What the sources say
- Smiths Metal Centres calls 3003 a medium-strength alloy about 20 percent stronger than 1100 with very good corrosion resistance, workability and weldability. 1
Things to know
- Only the O condition has two sources; the strain-hardened tempers (H12 to H18) come from the Aircraft Materials table alone. None is a design value.
Sources
- Smiths Metal Centres: 3003 Aluminium Technical Datasheet smithmetal.com/pdf/aluminium/3xxx/3003.pdf (distributor or reference site; read 2026-11-17)
- Aircraft Materials (UK stockist): Aluminium Alloy 3003 Technical Data Sheet aircraftmaterials.com/data/aluminium/3003.html (distributor or reference site; read 2026-11-17)
Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.