5083 aluminum
Properties of 5083 aluminum, each value tied to a recorded source.
The strongest of the common non-heat-treatable aluminum alloys, known for seawater resistance and for keeping its strength after welding. It is used for ships, pressure vessels and truck bodies, but it should not be used where it stays warmer than about 65 °C.
Composition
Weight percent. The two sources agree on every limit.
| Element | Limits | Source |
|---|---|---|
| Silicon (Si) | 0.40 max | 2,1 |
| Iron (Fe) | 0.40 max | 2,1 |
| Copper (Cu) | 0.10 max | 2,1 |
| Manganese (Mn) | 0.40 to 1.00 | 2,1 |
| Magnesium (Mg) | 4.00 to 4.90 | 2,1 |
| Chromium (Cr) | 0.05 to 0.25 | 2,1 |
| Zinc (Zn) | 0.25 max | 2,1 |
| Titanium (Ti) | 0.15 max | 2,1 |
| Aluminum (Al) | balance | 2,1 |
Properties
| Property | SI | US customary | Basis | Source |
|---|---|---|---|---|
| Physical | ||||
| Density | 2.650 g/cm³ | 0.0957 lb/in³ | typical, O/H111 | 1 |
| Mechanical | ||||
| Elastic modulus (Young's) | 72.0 GPa | 10.4 Msi | typical, O/H111 | 1 |
| Yield strength | 145 MPa | 21.0 ksi | typical, proof stress, soft O/H111 | 1 |
| Yield strength | 110 MPa | 16.0 ksi | minimum, temper O, extruded bar under 5 in diameter (16 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 2 |
| Yield strength | 166 MPa | 24.0 ksi | minimum, temper H111, extruded bar under 5 in diameter (24 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 2 |
| Tensile strength (ultimate or at break) | 300 MPa | 43.5 ksi | typical, soft O/H111 | 1 |
| Tensile strength (ultimate or at break) | 269 MPa | 39.0 ksi | minimum, temper O, extruded bar under 5 in diameter (39 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 2 |
| Tensile strength (ultimate or at break) | 276 MPa | 40.0 ksi | minimum, temper H111, extruded bar under 5 in diameter (40 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 2 |
| Elongation at break | 23 % | typical, A50 mm, O/H111 | 1 | |
| Elongation at break | 14 % | minimum, in 2 in, temper O, extruded bar under 5 in diameter | 2 | |
| Elongation at break | 12 % | minimum, in 2 in, temper H111, extruded bar under 5 in diameter | 2 | |
| Shear strength | 175 MPa | 25.4 ksi | typical, O/H111 | 1 |
| Hardness, Vickers (HV) | 75 HV | typical, O/H111 | 1 | |
| Thermal | ||||
| Melting point (as published) | 570 °C | 1,058 °F | typical, published as a single melting point | 1 |
| Thermal conductivity | 121 W/m·K | 839 BTU·in/h·ft²·°F | typical, O/H111; temperature not stated | 1 |
| Thermal expansion (linear) | 25.0 µm/m·K | 13.9 µin/in·°F | typical, O/H111; temperature range not stated | 1 |
Specifications
- QQ-A-250/6: 5083 sheet and plate (listed as a similar specification) 2
What the sources say
- Smiths Metal Centres describes 5083 as highly resistant to seawater and industrial chemical attack, with the highest strength of the non-heat-treatable alloys, retaining exceptional strength after welding, and not recommended above 65 °C. 1
Things to know
- The two sources are on different bases: a typical set for the soft O/H111 condition and a table of minimums for extruded bar. None is a design value.
Sources
- Smiths Metal Centres: 5083 Aluminium Technical Datasheet smithmetal.com/pdf/aluminium/5xxx/5083.pdf (distributor or reference site; read 2026-11-17)
- Aircraft Materials (UK stockist): Aluminium Alloy 5083 Technical Data Sheet aircraftmaterials.com/data/aluminium/5083.html (distributor or reference site; read 2026-11-17)
Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.