6061-T6 aluminum
Properties of 6061-T6 aluminum, each value tied to a recorded source.
The most widely used general-purpose structural aluminum. It machines and welds well, resists corrosion, and is available in nearly every shape, which is why it is the default choice for brackets, frames, fixtures and enclosures.
Composition
Weight percent. The three sources agree on every limit.
| Element | Limits | Source |
|---|---|---|
| Silicon (Si) | 0.40 to 0.80 | 3,1,2 |
| Iron (Fe) | 0.70 max | 3,1,2 |
| Copper (Cu) | 0.15 to 0.40 | 3,1,2 |
| Manganese (Mn) | 0.15 max | 3,1,2 |
| Magnesium (Mg) | 0.80 to 1.20 | 3,1,2 |
| Chromium (Cr) | 0.04 to 0.35 | 3,1,2 |
| Zinc (Zn) | 0.25 max | 3,1,2 |
| Titanium (Ti) | 0.15 max | 3,1,2 |
| Aluminum (Al) | balance | 3,1,2 |
Properties
| Property | SI | US customary | Basis | Source |
|---|---|---|---|---|
| Physical | ||||
| Density | 2.700 g/cm³ | 0.0975 lb/in³ | typical, as published for 6061; temper not stated | 1 |
| Density | 2.700 g/cm³ | 0.0975 lb/in³ | typical, T6 extrusions | 2 |
| Mechanical | ||||
| Elastic modulus (Young's) | 70.0 GPa | 10.2 Msi | typical, as published for 6061; temper not stated | 1 |
| Elastic modulus (Young's) | 70.0 GPa | 10.2 Msi | typical, T6 extrusions | 2 |
| Yield strength | 241 MPa | 35.0 ksi | typical, T6 sheet and plate, 0.020 to 6.00 in thick (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 3 |
| Yield strength | 270 MPa | 39.2 ksi | typical, proof stress; temper not stated | 1 |
| Yield strength | 240 MPa | 34.8 ksi | minimum, proof stress; T6 extrusions up to 200 mm diameter, 5 mm wall for tube and profiles (BS EN 755-2:2008) | 2 |
| Tensile strength (ultimate or at break) | 290 MPa | 42.0 ksi | typical, T6 sheet and plate, 0.020 to 4.00 in thick (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 3 |
| Tensile strength (ultimate or at break) | 276 MPa | 40.0 ksi | typical, T6 plate, 4.00 to 6.00 in thick (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 3 |
| Tensile strength (ultimate or at break) | 310 MPa | 45.0 ksi | typical, temper not stated | 1 |
| Tensile strength (ultimate or at break) | 260 MPa | 37.7 ksi | minimum, T6 extrusions up to 200 mm diameter, 5 mm wall for tube and profiles (BS EN 755-2:2008) | 2 |
| Elongation at break | 10 % | typical, T6 sheet, 0.020 to 0.500 in thick | 3 | |
| Elongation at break | 9 % | typical, T6 sheet, 0.500 to 1.000 in thick | 3 | |
| Elongation at break | 8 % | typical, T6 sheet, 1.00 to 2.00 in thick | 3 | |
| Elongation at break | 6 % | typical, T6 plate, 2.00 to 6.00 in thick | 3 | |
| Elongation at break | 12 % | typical, 50 mm gauge length; temper not stated | 1 | |
| Hardness, Brinell (HB) | 95 HB | typical, Brinell, T6 extrusions | 2 | |
| Shear strength | 190 MPa | 27.6 ksi | typical, as published for 6061; temper not stated | 1 |
| Hardness, Vickers (HV) | 100 HV | typical, temper not stated | 1 | |
| Thermal | ||||
| Melting point (as published) | 650 °C | 1,202 °F | typical, published as a single melting point | 1 |
| Melting point (as published) | 650 °C | 1,202 °F | typical, published as a single melting point | 2 |
| Thermal conductivity | 166 W/m·K | 1,151 BTU·in/h·ft²·°F | typical, temperature not stated | 1 |
| Thermal conductivity | 166 W/m·K | 1,151 BTU·in/h·ft²·°F | typical, temperature not stated | 2 |
| Thermal expansion (linear) | 23.4 µm/m·K | 13.0 µin/in·°F | typical, temperature range not stated | 1 |
| Thermal expansion (linear) | 23.4 µm/m·K | 13.0 µin/in·°F | typical, temperature range not stated | 2 |
| Electrical | ||||
| Electrical resistivity | 40 nΩ·m | typical, T6 extrusions; printed as 0.040 x10^-6 ohm·m | 2 | |
Specifications
- AMS 4027: 6061-T6 sheet and T651 plate 3
- AMS 4117: 6061-T6/T651 cold finished bars, rod and wire 3
- AMS 4173: 6061-T6511 extrusion 3
- QQ-A-250/11: 6061 sheet and plate 3
- QQ-A-200/8: 6061-T6/T6511 extruded bar, tube and section 3
- EN 4213: 6061-T651 plate 3
Things to know
- The two sources give different strength numbers because they use different bases: the stockist lists 42 ksi tensile and 35 ksi yield for T6 (about 290 and 241 MPa) by thickness, while the distributor lists 310 and 270 MPa without naming a temper. A third source lists minimums for T6 extrusions (240 MPa proof, 260 MPa tensile, BS EN 755-2). None of these is a design value; use the specification and your material certificate.
- Strength drops sharply after welding (the heat-affected zone returns toward the annealed condition); design welded joints for the as-welded strength, not T6.
Sources
- Smiths Metal Centres: 6061 Aluminium Technical Datasheet smithmetal.com/pdf/aluminium/6xxx/6061.pdf (distributor or reference site; read 2026-11-17)
- Aalco Metals Limited: Aluminium Alloy, Commercial Alloy, 6061, T6 Extrusions (data per BS EN 573-3:2009 and BS EN 755-2:2008) aalco.co.uk/datasheets/Aluminium-Alloy-6061-T6-Extrusions_145.ashx (distributor or reference site; read 2026-11-17)
- Aircraft Materials (UK stockist): Aluminium Alloy 6061 Technical Data Sheet aircraftmaterials.com/data/aluminium/6061.html (distributor or reference site; read 2026-11-17)
Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.