6082-T6 aluminum

Properties of 6082-T6 aluminum, each value tied to a recorded source.

The European structural alloy, often used where North America uses 6061. It is the strongest of the 6000 series, machines and welds well and resists corrosion, so it suits machined parts, frames and structures.

Family
Aluminum alloys
Condition
T6: solution heat treated and artificially aged
Common forms
Bar, plate, sheet, tube and extrusions
Alloy
6082 (Al-Si-Mg-Mn)
EN
EN AW-6082 (AlSi1MgMn)
UNS
A96082
Relative cost
$$ Editorial, relative: similar to 6061 aluminum where it is stocked. Not a quote; prices change.

Composition

Weight percent. The magnesium range comes from Smiths; Aircraft Materials prints its lower limit as 0.06, which looks like a typo for 0.60.

ElementLimitsSource
Silicon (Si)0.70 to 1.302,1
Iron (Fe)0.50 max2,1
Copper (Cu)0.10 max2,1
Manganese (Mn)0.40 to 1.002,1
Magnesium (Mg)0.60 to 1.201
Chromium (Cr)0.25 max2,1
Aluminum (Al)balance2,1

Properties

PropertySIUS customaryBasisSource
Physical
Density2.700 g/cm³0.0975 lb/in³typical1
Mechanical
Elastic modulus (Young's)70.0 GPa10.2 Msitypical1
Yield strength255 MPa37.0 ksiminimum, T6 sheet and plate 0.2 to 3.0 mm; T6 bar under 20 mm2
Yield strength240 MPa34.8 ksiminimum, T6 sheet and plate 3.0 to 25 mm; T6 bar 150 to 200 mm2
Yield strength270 MPa39.2 ksiminimum, T6 bar 20 to 150 mm2
Tensile strength (ultimate or at break)295 MPa42.8 ksiminimum, T6 sheet and plate 0.2 to 25 mm; T6 bar under 20 mm2
Tensile strength (ultimate or at break)310 MPa45.0 ksiminimum, T6 bar 20 to 150 mm2
Tensile strength (ultimate or at break)280 MPa40.6 ksiminimum, T6 bar 150 to 200 mm2
Elongation at break8 %minimum, T6 sheet, plate and bar under 150 mm (on 50 mm or 5.65 times the root of the area)2
Elongation at break5 %minimum, T6 bar 150 to 200 mm2
Thermal
Melting point (as published)555 °C1,031 °Ftypical, published as a single melting point1
Thermal conductivity180 W/m·K1,248 BTU·in/h·ft²·°Ftypical, temperature not stated1
Thermal expansion (linear)24.0 µm/m·K13.3 µin/in·°Ftypical, temperature range not stated1

Specifications

  • EN 2326: 6082-T6 extruded bar (listed as a similar specification) 2
  • BS L115: 6082-T651 plate (listed as a similar specification) 2

What the sources say

  • Smiths Metal Centres describes 6082 as the highest-strength alloy of the 6000 series, often called a structural alloy, and rates its corrosion resistance as good. 1

Things to know

  • Strengths are minimums from one stockist's table (EN-style limits by thickness). The Smiths sheet gives typical strengths without naming a temper, so they are not used here.
  • Minimums fall slightly for thicker sections.

Sources

  1. Smiths Metal Centres: 6082 Aluminium Technical Datasheet smithmetal.com/pdf/aluminium/6xxx/6082.pdf (distributor or reference site; read 2026-11-17)
  2. Aircraft Materials (UK stockist): Aluminium Alloy 6082 Technical Data Sheet aircraftmaterials.com/data/aluminium/6082.html (distributor or reference site; read 2026-11-17)

Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.

All materials

Published by Nick Peterson, mechanical engineer.