ABS

Properties of ABS, each value tied to a recorded source.

A general-purpose ABS: tough, reasonably stiff, with better heat resistance than PLA, which is why it is the classic housing plastic. It prints with more warping and fumes than PLA or PETG and needs an enclosure, but it sands, glues and vapor-smooths well.

Family
Plastics: ABS (acrylonitrile butadiene styrene)
Condition
Typical values for uncolored molded specimens of one general-purpose grade (ISO methods), not printed parts
Common forms
Resin pellets for injection molding; ABS filament makers use similar grades
Manufacturer grade
TERLURAN GP-22 (INEOS Styrolution)
Polymer
Acrylonitrile butadiene styrene (ABS)
Relative cost
$ Editorial, relative: among the cheapest common prototyping plastics per kilogram. Not a quote; prices change.

Properties

PropertySIUS customaryBasisSource
Physical
Density1.040 g/cm³0.0376 lb/in³typical, ISO 1183 (Printed as 1040 kg/m³.)1
Water absorption1.00 %typical, saturated at 23 °C, ISO 621
Water absorption0.220 %typical, equilibrium at 23 °C and 50 % RH, ISO 621
Mechanical
Elastic modulus (Young's)2.3 GPa0.334 Msitypical, tensile, ISO 527 (Printed as 2300 MPa.)1
Yield strength45 MPa6.53 ksitypical, tensile stress at yield, 23 °C, ISO 5271
Elongation at break10 %typical, nominal strain at break, 23 °C, ISO 5271
Flexural strength65 MPa9.43 ksitypical, 23 °C, ISO 1781
Notched Izod impact (ISO)26.0 kJ/m²typical, notched, 23 °C, ISO 180/A1
Notched Izod impact (ISO)8.0 kJ/m²typical, notched, -30 °C, ISO 180/A1
Notched Charpy impact (ISO)22.0 kJ/m²typical, notched, 23 °C, ISO 179/1eA1
Notched Charpy impact (ISO)8.0 kJ/m²typical, notched, -30 °C, ISO 179/1eA1
Thermal
Thermal conductivity0.170 W/m·K1.18 BTU·in/h·ft²·°Ftypical, ISO 22007-41
Thermal expansion (linear)80.0 to 110.0 µm/m·K44.4 to 61.1 µin/in·°Frange, ISO 113591
Heat deflection temperature94 °C201 °Ftypical, at 1.8 MPa, annealed 4 h at 80 °C, ISO 75 (method A)1
Heat deflection temperature99 °C210 °Ftypical, at 0.45 MPa, annealed 4 h at 80 °C, ISO 75 (method B)1
Vicat softening temperature96 °C205 °Ftypical, VST/B/50 (50 N, 50 °C/h), ISO 3061
Vicat softening temperature105 °C221 °Ftypical, VST/A/50 (10 N, 50 °C/h), ISO 3061
Processing
Processing melt temperature220 to 260 °C428 to 500 °Frange, melt temperature range for injection molding, ISO 2941

What the sources say

  • INEOS Styrolution gives drying at 80 °C for 2 to 4 hours before processing. 1
  • INEOS Styrolution describes the grade as an easy-flow, general-purpose injection molding material with high resistance to impact and heat distortion, aimed mainly at housings. 1

Things to know

  • This is one injection-molding grade. 3D-printing ABS filaments differ by maker, and printed parts are weaker across layers than the molded values here.
  • The heat deflection temperatures here are for specimens annealed 4 hours at 80 °C, which raises them above an unannealed part.

Sources

  1. INEOS Styrolution: TERLURAN GP-22 Technical Data Sheet, ISO version (typical values for uncolored products; revision date 08/01/2022) eshop.ineos-styrolution.com/Product/Terluran_TERLURAN-GP-22_SKU300600120827.html (the maker of the material; read 2026-11-17)

Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.

All materials