Free-machining brass CZ121 (CW614N)

Properties of Free-machining brass CZ121 (CW614N), each value tied to a recorded source.

The standard free-machining brass: it cuts cleanly with short chips at high speed, which is why other metals' machinability is rated against it. It contains lead, is not suited to cold forming, and is used for fittings, fixtures, bushings and decorative machined parts.

Family
Copper alloys: brass
Condition
Bar; strength depends on size and temper
Common forms
Round, flat, square and hexagon bar
EN
CW614N (CZ121)
UNS
C38500 (per the source, not a direct equivalent)
Symbol
CuZn39Pb3
Relative cost
$$ Editorial, relative: more than aluminum and mild steel, less than copper and stainless steel. Not a quote; prices change.

Composition

Weight percent per EN 12164:2011 as listed by the source.

ElementLimitsSource
Copper (Cu)57.00 to 59.001
Lead (Pb)2.50 to 3.501,2
Aluminum (Al)0.05 max1
Iron (Fe)0.30 max1,2
Nickel (Ni)0.30 max1
Tin (Sn)0.30 max1
Zinc (Zn)balance1

Properties

PropertySIUS customaryBasisSource
Physical
Density8.470 g/cm³0.306 lb/in³typical1
Mechanical
Elastic modulus (Young's)97.0 GPa14.1 Msitypical1
Yield strength230 to 350 MPa33.4 to 50.8 ksirange, proof stress, bar 6 to 80 mm1
Tensile strength (ultimate or at break)360 to 500 MPa52.2 to 72.5 ksirange, bar 6 to 80 mm1
Tensile strength (ultimate or at break)360 to 580 MPa52.2 to 84.1 ksirange, bar, temper not stated2
Elongation at break5 to 20 %range, A, bar 6 to 80 mm (printed as 20 to 5)1
Elongation at break15 to 25 %range, bar, temper not stated2
Hardness, Brinell (HB)90 to 160 HBrange, Brinell, bar 6 to 80 mm1
Thermal
Melting point (as published)875 °C1,607 °Ftypical, published as a single melting point1
Thermal conductivity123 W/m·K853 BTU·in/h·ft²·°Ftypical, temperature not stated1
Thermal expansion (linear)20.9 µm/m·K11.6 µin/in·°Ftypical, temperature range not stated1
Electrical
Electrical resistivity62 nΩ·mtypical, printed as 0.062 x10^-6 ohm·m1

What the sources say

  • The source rates machinability as excellent, with a rating of 100 (the standard other alloys are measured against), cold working as poor and not recommended, hot working as excellent between 630 and 730 °C, and soldering as excellent. 1

Things to know

  • Two distributor sources (Aalco, EN 12164 CW614N, and Smiths, CZ121). Smiths lists copper as 56.5 to 58.5 percent against Aalco's 57 to 59, so copper is shown from Aalco only; lead and iron agree. Strength ranges depend on temper and bar size.

Sources

  1. Aalco Metals Limited: Copper and Copper Alloys, Brass, CW614N Brass Rod (data per EN 12164:2011) aalco.co.uk/datasheets/Copper-and-Copper-Alloys-CW614N-Brass-Rod_31.ashx (distributor or reference site; read 2026-11-17)
  2. Smiths Metal Centres: CZ121 Brass Technical Datasheet smithmetal.com/pdf/brass/cz121.pdf (distributor or reference site; read 2026-11-17)

Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.