Nylon 12 (PA12)
Properties of Nylon 12 (PA12), each value tied to a recorded source.
A light, tough nylon that absorbs much less water than nylon 6 (about 1.6 percent at saturation here), so its stiffness and strength change little between dry and conditioned states. This rigid natural grade is made for extruding tubing.
Properties
| Property | SI | US customary | Basis | Source |
|---|---|---|---|---|
| Physical | ||||
| Density | 1.010 g/cm³ | 0.0365 lb/in³ | typical, 23 °C, ISO 1183-1 | 1 |
| Water absorption | 1.60 % | typical, equilibrium, immersion at 23 °C, ISO 62 | 1 | |
| Mechanical | ||||
| Elastic modulus (Young's) | 1.5 GPa | 0.218 Msi | typical, tensile, 23 °C, dry, ISO 527-1/-2 (Printed as 1500 MPa.) | 1 |
| Elastic modulus (Young's) | 1.4 GPa | 0.209 Msi | typical, tensile, 23 °C, conditioned (Printed as 1440 MPa.) | 1 |
| Yield strength | 50 MPa | 7.25 ksi | typical, yield stress, 23 °C, dry, ISO 527-1/-2 (yield strain 5 %) | 1 |
| Yield strength | 43 MPa | 6.24 ksi | typical, yield stress, 23 °C, conditioned (yield strain 5 %) | 1 |
| Tensile strength (ultimate or at break) | 47 MPa | 6.82 ksi | typical, stress at break, 23 °C, conditioned, ISO 527-1/-2 (no dry value printed) | 1 |
| Elongation at break | 50 % | minimum, nominal strain at break, 23 °C, dry and conditioned (printed as > 50) | 1 | |
| Flexural modulus | 1.2 GPa | 0.178 Msi | typical, 23 °C, conditioned, ISO 178 (no dry value printed) (Printed as 1230 MPa.) | 1 |
| Notched Charpy impact (ISO) | 11.0 kJ/m² | typical, notched, 23 °C, conditioned, ISO 179 1eA | 1 | |
| Notched Charpy impact (ISO) | 6.0 kJ/m² | typical, notched, -30 °C, conditioned, ISO 179 1eA | 1 | |
| Thermal | ||||
| Melting point (as published) | 180 °C | 356 °F | typical, melting temperature, 10 °C/min, ISO 11357-1/-3 | 1 |
| Heat deflection temperature | 55 °C | 131 °F | typical, at 1.8 MPa, ISO 75-1/-2 | 1 |
| Heat deflection temperature | 135 °C | 275 °F | typical, at 0.45 MPa, ISO 75-1/-2 | 1 |
| Vicat softening temperature | 142 °C | 288 °F | typical, 50 N at 50 °C/h, ISO 306 | 1 |
| Processing | ||||
| Processing melt temperature | 230 to 270 °C | 446 to 518 °F | range, injection molding melt temperature, min to max (250 °C recommended) | 1 |
Things to know
- Dry means dry as molded; conditioned means after conditioning (the sheet does not print the humidity). Several properties are printed only for the conditioned state.
- Unnotched Charpy is printed as no break at 23 °C and -30 °C (conditioned). Melt volume rate is 8 cm³/10 min at 235 °C/5 kg (a volume rate, so not entered as melt flow rate). Burning behavior is HB75 at 1.5 mm and HB40 at 3.0 mm.
- The volume resistivity (1.0E+12 ohm.m, conditioned) is outside the range this library can show and is left out. Plasticized PA12 grades and PA12 powders for 3D printing differ; use that product's own data.
Sources
- Arkema: RILSAMID AESNO TL Technical Data Sheet, polyamide 12 pellet (English, worldwide; page footer HPP - 2026-11-07) hpp.arkema.com/assets/arkema/TDS_RILSAMID%C2%AE%20AESNO%20TL_en_WW.pdf (the maker of the material; read 2026-11-17)
Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.