Nylon 66 (PA66)
Properties of Nylon 66 (PA66), each value tied to a recorded source.
A tough, wear-resistant engineering plastic used for gears, bearings and sliding parts. It is strong and handles heat well for a plastic, but it absorbs water, which makes it softer and larger, so the dry and conditioned values below differ a lot.
Properties
| Property | SI | US customary | Basis | Source |
|---|---|---|---|---|
| Physical | ||||
| Density | 1.130 g/cm³ | 0.0408 lb/in³ | typical, ISO 1183 (Printed as 1130 kg/m³.) | 1 |
| Water absorption | 8.00 to 9.00 % | range, saturation in water at 23 °C (similar to ISO 62) | 1 | |
| Water absorption | 2.50 to 3.10 % | range, equilibrium at 23 °C and 50 % RH (similar to ISO 62) | 1 | |
| Mechanical | ||||
| Elastic modulus (Young's) | 3.0 GPa | 0.435 Msi | typical, tensile, dry, ISO 527-1/-2 (Printed as 3000 MPa.) | 1 |
| Elastic modulus (Young's) | 1.1 GPa | 0.160 Msi | typical, tensile, conditioned, ISO 527-1/-2 (Printed as 1100 MPa.) | 1 |
| Yield strength | 85 MPa | 12.3 ksi | typical, yield stress, dry, 50 mm/min, ISO 527-1/-2 | 1 |
| Yield strength | 50 MPa | 7.25 ksi | typical, yield stress, conditioned, 50 mm/min, ISO 527-1/-2 | 1 |
| Elongation at break | 30 % | typical, nominal strain at break, dry, ISO 527-1/-2 (conditioned is printed as above 50) | 1 | |
| Flexural modulus | 2.9 GPa | 0.421 Msi | typical, dry, ISO 178 (Printed as 2900 MPa.) | 1 |
| Notched Charpy impact (ISO) | 5.0 kJ/m² | typical, notched, 23 °C, dry, ISO 179/1eA | 1 | |
| Notched Charpy impact (ISO) | 20.0 kJ/m² | typical, notched, 23 °C, conditioned, ISO 179/1eA | 1 | |
| Notched Charpy impact (ISO) | 4.0 kJ/m² | typical, notched, -30 °C, dry, ISO 179/1eA | 1 | |
| Thermal | ||||
| Melting point (as published) | 260 °C | 500 °F | typical, melting temperature, DSC, ISO 11357-1/-3 | 1 |
| Thermal conductivity | 0.330 W/m·K | 2.29 BTU·in/h·ft²·°F | typical, DIN 52612-1 | 1 |
| Specific heat | 1.700 J/g·K | 0.406 BTU/lb·°F | typical (Printed as 1700 J/(kg·K).) | 1 |
| Thermal expansion (linear) | 98.0 µm/m·K | 54.4 µin/in·°F | typical, longitudinal, 23 to 55 °C, ISO 11359-1/-2 | 1 |
| Heat deflection temperature | 75 °C | 167 °F | typical, at 1.8 MPa (HDT A), ISO 75-1/-2 | 1 |
| Heat deflection temperature | 220 °C | 428 °F | typical, at 0.45 MPa (HDT B), ISO 75-1/-2 | 1 |
| Maximum service temperature | 200 °C | 392 °F | typical, short cycle operation | 1 |
| Processing | ||||
| Processing melt temperature | 280 to 300 °C | 536 to 572 °F | range, melt temperature, injection molding and extrusion | 1 |
What the sources say
- BASF describes Ultramid A3K as an easy-flowing injection-molding grade for fast processing, used for highly stressed technical parts such as bearings and gear wheels, and says the containers should be opened only immediately before processing or drying because the granules absorb moisture. 1
Things to know
- Dry and conditioned (humid) values differ strongly: yield stress falls from 85 to 50 MPa and tensile modulus from 3.0 to 1.1 GPa. Design for the conditioned state unless the part stays dry.
- The sheet's values are for one molded grade. Nylon filaments for 3D printing (often PA6 or PA12 blends) and cast or extruded nylon stock differ; check that product's own data.
Sources
- BASF SE: Ultramid A3K Product Information (PA66), Asia Pacific / Europe, English (sheet dated 09/2026) download.basf.com/p1/8a8082587fd4b608017fd64108ab6d3b/en/ULTRAMID_A3K_Product_Data_Sheet_Asia_PacificEurope_English.pdf (the maker of the material; read 2026-11-17)
Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.