PETG (glycol-modified polyester)

Properties of PETG (glycol-modified polyester), each value tied to a recorded source.

A clear, tough, amorphous copolyester of the kind sold as PETG. It is easier to print than ABS, tougher than PLA and fairly stiff, with moderate heat resistance, which makes it a good all-round prototype plastic for functional parts, covers and fluid-contact parts at modest temperatures.

Family
Plastics: PETG (glycol-modified polyester)
Condition
Typical values for injection-molded specimens of one maker's resin, not 3D-printed parts and not any filament brand
Common forms
Resin pellets for molding and extrusion; PETG filament makers use similar copolyesters
Manufacturer grade
Eastar copolyester 6763 (Eastman Chemical Company)
Relative cost
$ Editorial, relative: similar to PLA and ABS per kilogram, below nylon and polycarbonate. Not a quote; prices change.

Properties

PropertySIUS customaryBasisSource
Physical
Density1.270 g/cm³0.0459 lb/in³typical, ASTM D792 (specific gravity)1
Water absorption0.130 %typical, 24 h immersion, ASTM D5701
Mechanical
Elastic modulus (Young's)2.1 GPa0.305 Msitypical, tensile, ASTM D638 (Printed as 2100 MPa.)1
Yield strength50 MPa7.25 ksitypical, tensile stress at yield, ASTM D638 (7,300 psi)1
Tensile strength (ultimate or at break)28 MPa4.06 ksitypical, tensile stress at break, ASTM D638 (4,100 psi)1
Elongation at break130 %typical, at break, ASTM D638 (the sheet lists 100 percent by ISO 527)1
Flexural strength70 MPa10.2 ksitypical, flexural yield strength, ASTM D790 (10,200 psi)1
Flexural modulus2.1 GPa0.305 Msitypical, ASTM D790 (Printed as 2100 MPa.)1
Notched Izod impact101 J/m1.89 ft·lb/intypical, notched, 23 °C, ASTM D256 (1.9 ft·lbf/in)1
Notched Izod impact37 J/m0.693 ft·lb/intypical, notched, -40 °C, ASTM D256 (0.7 ft·lbf/in)1
Hardness, Rockwell R106 HRRtypical, Rockwell R scale, ASTM D7851
Thermal
Thermal conductivity0.210 W/m·K1.46 BTU·in/h·ft²·°Ftypical, ASTM C1771
Specific heat1.760 J/g·K0.420 BTU/lb·°Ftypical, 100 °C, DSC (Printed as 1.76 kJ/kg·K.)1
Thermal expansion (linear)51.0 µm/m·K28.3 µin/in·°Ftypical, ASTM D696 (Printed as 5.1 x 10^-5 per °C.)1
Glass transition temperature80 °C176 °Ftypical, DSC1
Heat deflection temperature70 °C158 °Ftypical, at 0.455 MPa (66 psi), ASTM D6481
Heat deflection temperature64 °C147 °Ftypical, at 1.82 MPa (264 psi), ASTM D6481
Vicat softening temperature85 °C185 °Ftypical, ASTM D15251
Processing
Processing melt temperature249 to 271 °C480 to 520 °Frange, typical processing melt temperature (for molding and extrusion)1

What the sources say

  • Eastman gives drying conditions of 65 °C (150 °F) for 4 to 6 hours before processing. 1
  • Eastman describes Eastar 6763 as a clear, amorphous material that molds and extrudes easily, with excellent clarity and toughness, meeting ISO 10993 and/or USP Class VI biocompatibility requirements and food-contact status for the resin as sold. 1

Things to know

  • This is one maker's medical-packaging resin. Filament makers use their own copolyester resins and additives, so a given PETG filament can differ noticeably in heat resistance and strength. Check the filament maker's data sheet when it matters.
  • Printed parts are weaker than molded specimens, especially across layers.

Sources

  1. Eastman Chemical Company: Eastar copolyester 6763 Technical Data Sheet (Typical Properties) productcatalog.eastman.com/tds/ProdDatasheet.aspx?product=71040786&pn=Eastar+Copolyester+6763 (the maker of the material; read 2026-11-17)

Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.

All materials

Published by Nick Peterson, mechanical engineer.