Polycarbonate (PC)

Properties of Polycarbonate (PC), each value tied to a recorded source.

A very tough, clear engineering plastic with high heat resistance for a thermoplastic. It is the choice for impact-resistant covers, guards and clear housings, but it is harder to print and to machine without cracking than the common hobby plastics and absorbs moisture that must be dried out before processing.

Family
Plastics: PC (polycarbonate)
Condition
Typical values for molded specimens of one low-viscosity UV-stabilized grade, not machined or printed parts
Common forms
Resin pellets for injection molding; sheet and rod are made from similar grades
Manufacturer grade
Makrolon 2407 (Covestro)
Polymer
Polycarbonate (PC)
Relative cost
$$ Editorial, relative: more than ABS, PETG and PLA, similar to nylon. Not a quote; prices change.

Properties

PropertySIUS customaryBasisSource
Physical
Density1.200 g/cm³0.0434 lb/in³typical, ISO 1183-1 (Printed as 1200 kg/m³.)1
Water absorption0.300 %typical, saturation value, water at 23 °C, ISO 621
Water absorption0.120 %typical, equilibrium value, 23 °C and 50 % RH, ISO 621
Mechanical
Elastic modulus (Young's)2.4 GPa0.348 Msitypical, tensile, 1 mm/min, ISO 527-1,-2 (Printed as 2400 MPa.)1
Yield strength66 MPa9.57 ksitypical, yield stress, 50 mm/min, ISO 527-1,-21
Tensile strength (ultimate or at break)65 MPa9.43 ksitypical, stress at break, 50 mm/min, ISO 527-1,-21
Elongation at break120 %typical, strain at break, 50 mm/min, ISO 527-1,-21
Flexural strength98 MPa14.2 ksitypical, ISO 1781
Flexural modulus2.4 GPa0.341 Msitypical, ISO 178 (Printed as 2350 MPa.)1
Notched Izod impact (ISO)65.0 kJ/m²typical, notched, 23 °C, 3 mm, ISO 21305 / based on ISO 180/A1
Notched Izod impact (ISO)12.0 kJ/m²typical, notched, -30 °C, 3 mm, ISO 21305 / based on ISO 180/A1
Notched Charpy impact (ISO)14.0 kJ/m²typical, notched, -30 °C, 3 mm, ISO 179-1/1eA1
Thermal
Thermal conductivity0.200 W/m·K1.39 BTU·in/h·ft²·°Ftypical, through-plane, 23 °C and 50 % RH, ISO 83021
Thermal expansion (linear)65.0 µm/m·K36.1 µin/in·°Ftypical, 23 to 55 °C, parallel and normal, ISO 11359-1,-2 (Printed as 0.65 x 10^-4 per K.)1
Glass transition temperature143 °C289 °Ftypical, 10 °C/min, ISO 11357-1,-21
Heat deflection temperature136 °C277 °Ftypical, at 0.45 MPa, ISO 75-1,-21
Heat deflection temperature124 °C255 °Ftypical, at 1.80 MPa, ISO 75-1,-21
Vicat softening temperature143 °C289 °Ftypical, 50 N; 50 °C/h, ISO 3061
Vicat softening temperature145 °C293 °Ftypical, 50 N; 120 °C/h, ISO 3061
Processing
Melt flow rate20 g/10 mintypical, 300 °C / 1.2 kg, ISO 1133-11
Processing melt temperature280 to 320 °C536 to 608 °Frange, recommended melt temperature (standard 300 °C)1

What the sources say

  • Covestro recommends dry-air drying at 120 °C for 2 to 3 hours to a moisture content of 0 to 0.02 percent before processing. 1
  • Covestro lists the burning behavior as UL 94 V-2 at 0.75 mm and HB at 2.7 mm. 1

Things to know

  • Typical values for one injection-molding grade. Extruded sheet, machined parts and 3D-printed polycarbonate use different grades and processes; check that product's own data.

Sources

  1. Covestro: Makrolon 2407 product page, Typical values (polycarbonate) solutions.covestro.com/en/products/makrolon/makrolon-2407_000000000086286874 (the maker of the material; read 2026-11-17)

Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.

All materials