17-4 PH stainless steel (EN 1.4542)
Properties of 17-4 PH stainless steel (EN 1.4542), each value tied to a recorded source.
A precipitation hardening stainless steel with about 17 percent chromium, 4 percent nickel and 4 percent copper. It is machined in the solution annealed condition and then hardened by a single low-temperature aging treatment, which gives high strength with little distortion. Strength and hardness depend on the aging condition, from H900 (strongest) to H1150 (lowest strength, highest elongation).
Composition
Weight percent, AMS 5643 limits as printed by Smiths and Aircraft Materials. Aalco prints the EN 10088-3 limits for 1.4542, which differ for chromium (15.00 to 17.00), manganese (1.50), silicon (0.70) and molybdenum (0.60), so Aalco is cited only on the rows it agrees with. Niobium also has a minimum of 5 times the carbon content (Smiths; Aircraft Materials gives it for niobium plus tantalum). Aircraft Materials lists no molybdenum limit.
| Element | Limits | Source |
|---|---|---|
| Carbon (C) | 0.07 max | 3,2,1 |
| Chromium (Cr) | 15.00 to 17.50 | 3,2 |
| Nickel (Ni) | 3.00 to 5.00 | 3,2,1 |
| Copper (Cu) | 3.00 to 5.00 | 3,2,1 |
| Manganese (Mn) | 1.00 max | 3,2 |
| Silicon (Si) | 1.00 max | 3,2 |
| Phosphorus (P) | 0.04 max | 3,2,1 |
| Sulfur (S) | 0.03 max | 3,2,1 |
| Niobium (Nb) | 0.45 max | 3,2,1 |
| Molybdenum (Mo) | 0.50 max | 2 |
| Iron (Fe) | balance | 1 |
Properties
| Property | SI | US customary | Basis | Source |
|---|---|---|---|---|
| Physical | ||||
| Density | 7.750 g/cm³ | 0.280 lb/in³ | typical | 1 |
| Density | 7.750 g/cm³ | 0.280 lb/in³ | typical, printed as 7.75 kg/dm³ | 2 |
| Mechanical | ||||
| Elastic modulus (Young's) | 196.0 GPa | 28.4 Msi | typical | 1 |
| Yield strength | 1,172 MPa | 170 ksi | typical, H900, 0.2 % proof stress | 2 |
| Yield strength | 1,069 MPa | 155 ksi | typical, H925, 0.2 % proof stress | 2 |
| Yield strength | 1,000 MPa | 145 ksi | typical, H1025, 0.2 % proof stress | 2 |
| Yield strength | 862 MPa | 125 ksi | typical, H1075, 0.2 % proof stress | 2 |
| Yield strength | 793 MPa | 115 ksi | typical, H1100, 0.2 % proof stress | 2 |
| Yield strength | 724 MPa | 105 ksi | typical, H1150, 0.2 % proof stress | 2 |
| Yield strength | 1,172 MPa | 170 ksi | typical, H900, 0.2 % yield (170 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 3 |
| Yield strength | 1,069 MPa | 155 ksi | typical, H925, 0.2 % yield (155 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 3 |
| Yield strength | 1,000 MPa | 145 ksi | typical, H1025, 0.2 % yield (145 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 3 |
| Yield strength | 862 MPa | 125 ksi | typical, H1075, 0.2 % yield (125 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 3 |
| Yield strength | 793 MPa | 115 ksi | typical, H1100, 0.2 % yield (115 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 3 |
| Yield strength | 724 MPa | 105 ksi | typical, H1150, 0.2 % yield (105 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 3 |
| Yield strength | 520 MPa | 75.4 ksi | minimum, P800, proof stress, bar up to 100 mm | 1 |
| Yield strength | 720 MPa | 104 ksi | minimum, P930, proof stress, bar up to 100 mm | 1 |
| Yield strength | 790 MPa | 115 ksi | minimum, P960, proof stress, bar up to 100 mm | 1 |
| Yield strength | 1,000 MPa | 145 ksi | minimum, P1070, proof stress, bar up to 100 mm | 1 |
| Tensile strength (ultimate or at break) | 1,310 MPa | 190 ksi | typical, H900 | 2 |
| Tensile strength (ultimate or at break) | 1,172 MPa | 170 ksi | typical, H925 | 2 |
| Tensile strength (ultimate or at break) | 1,069 MPa | 155 ksi | typical, H1025 | 2 |
| Tensile strength (ultimate or at break) | 1,000 MPa | 145 ksi | typical, H1075 | 2 |
| Tensile strength (ultimate or at break) | 965 MPa | 140 ksi | typical, H1100 | 2 |
| Tensile strength (ultimate or at break) | 931 MPa | 135 ksi | typical, H1150 | 2 |
| Tensile strength (ultimate or at break) | 1,310 MPa | 190 ksi | typical, H900 (190 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 3 |
| Tensile strength (ultimate or at break) | 1,172 MPa | 170 ksi | typical, H925 (170 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 3 |
| Tensile strength (ultimate or at break) | 1,069 MPa | 155 ksi | typical, H1025 (155 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 3 |
| Tensile strength (ultimate or at break) | 1,000 MPa | 145 ksi | typical, H1075 (145 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 3 |
| Tensile strength (ultimate or at break) | 965 MPa | 140 ksi | typical, H1100 (140 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 3 |
| Tensile strength (ultimate or at break) | 931 MPa | 135 ksi | typical, H1150 (135 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 3 |
| Tensile strength (ultimate or at break) | 1,200 MPa | 174 ksi | maximum, solution annealed bar up to 100 mm | 1 |
| Tensile strength (ultimate or at break) | 800 to 950 MPa | 116 to 138 ksi | range, P800, bar up to 100 mm | 1 |
| Tensile strength (ultimate or at break) | 930 to 1,100 MPa | 135 to 160 ksi | range, P930, bar up to 100 mm | 1 |
| Tensile strength (ultimate or at break) | 960 to 1,160 MPa | 139 to 168 ksi | range, P960, bar up to 100 mm | 1 |
| Tensile strength (ultimate or at break) | 1,070 to 1,270 MPa | 155 to 184 ksi | range, P1070, bar up to 100 mm | 1 |
| Elongation at break | 10 % | typical, H900, on 4D gauge length | 2 | |
| Elongation at break | 10 % | typical, H925, on 4D gauge length | 2 | |
| Elongation at break | 12 % | typical, H1025, on 4D gauge length | 2 | |
| Elongation at break | 13 % | typical, H1075, on 4D gauge length | 2 | |
| Elongation at break | 14 % | typical, H1100, on 4D gauge length | 2 | |
| Elongation at break | 16 % | typical, H1150, on 4D gauge length | 2 | |
| Elongation at break | 10 % | typical, H900, in 2D | 3 | |
| Elongation at break | 10 % | typical, H925, in 2D | 3 | |
| Elongation at break | 12 % | typical, H1025, in 2D | 3 | |
| Elongation at break | 13 % | typical, H1075, in 2D | 3 | |
| Elongation at break | 14 % | typical, H1100, in 2D | 3 | |
| Elongation at break | 16 % | typical, H1150, in 2D | 3 | |
| Elongation at break | 18 % | minimum, P800, A, bar up to 100 mm | 1 | |
| Elongation at break | 16 % | minimum, P930, A, bar up to 100 mm | 1 | |
| Elongation at break | 12 % | minimum, P960, A, bar up to 100 mm | 1 | |
| Elongation at break | 10 % | minimum, P1070, A, bar up to 100 mm | 1 | |
| Hardness, Brinell (HB) | 388 to 444 HB | range, H900 | 2 | |
| Hardness, Brinell (HB) | 375 to 429 HB | range, H925 | 2 | |
| Hardness, Brinell (HB) | 331 to 401 HB | range, H1025 | 2 | |
| Hardness, Brinell (HB) | 311 to 375 HB | range, H1075 | 2 | |
| Hardness, Brinell (HB) | 302 to 363 HB | range, H1100 | 2 | |
| Hardness, Brinell (HB) | 277 to 352 HB | range, H1150 | 2 | |
| Hardness, Brinell (HB) | 363 HB | maximum, condition A (solution annealed) | 3 | |
| Hardness, Brinell (HB) | 360 HB | maximum, solution annealed bar up to 100 mm | 1 | |
| Thermal | ||||
| Thermal conductivity | 18 W/m·K | 128 BTU·in/h·ft²·°F | typical, temperature not stated | 1 |
| Thermal expansion (linear) | 10.8 µm/m·K | 6.00 µin/in·°F | typical, temperature range not stated | 1 |
| Electrical | ||||
| Electrical resistivity | 800 nΩ·m | typical, printed as 0.8 x10^-6 ohm·m | 1 | |
Specifications
- AMS 5643: bars, wire, forgings, tubing and rings 3
- AMS 5604: sheet, strip and plate 3
- ASTM A564 Grade 630: listed as a specification (with ASME SA564) 3
- ASME SA-564 Type 630: listed as a related specification 2
- EN 10088-3:2005: composition and bar properties for 1.4542 (as cited by Aalco) 1
What the sources say
- Smiths Metal Centres says the material should not be used in the annealed condition, that its corrosion resistance is superior to straight chromium grades like 410 and approaches the chromium-nickel grades, and that it is readily weldable without the pre-heat and post-heat used for other hardenable stainless grades. 2
- Aalco says the corrosion resistance is similar to grade 304, that 17-4 PH is susceptible to pitting and crevice corrosion in warm chloride environments, and that parts shrink slightly when aged: about 0.05 percent for H900 and 0.10 percent for H1150. 1
- Aalco advises against prolonged exposure to 370 to 480 °C where toughness at room temperature matters, and against use above the precipitation hardening temperature. 1
Things to know
- Three distributor sources; all disclaim their data (indicative, approximate or guideline only), so confirm against the specification and your material certificate. Strength depends on the aging condition: H900 is the strongest and H1150 the most ductile.
- Smiths and Aircraft Materials both label their H-condition values as typical and agree once the ksi values are converted. Aalco gives EN 10088-3 minimums and ranges for the P800 to P1070 conditions, which are different heat treatments from the H conditions, so they are listed separately.
- The Aircraft Materials bar table heads its hardness column "Rockwell C" but prints Brinell-like numbers (388-444 and so on), so its H-condition hardness is not used; Smiths gives the same ranges as Brinell. Aircraft Materials also gives sheet hardness in Rockwell C, which this library has no field for.
- Aalco's Heat Treatment section shows a QT 650 to QT 900 tensile list that does not match this grade's conditions, so it is not used.
Sources
- Aalco Metals Limited: Stainless Steel, Precipitation Hardening, 1.4542 (17/4 and 630) Bar (data per EN 10088-3:2005) aalco.co.uk/datasheets/Stainless-Steel-14542-174--630-Bar_100.ashx (distributor or reference site; read 2026-11-17)
- Smiths Metal Centres: AMS 5643 (17/4 PH) Precipitation Hardening Stainless Steel Bar Technical Datasheet smithmetal.com/pdf/stainless/ph/17-4ph.pdf (distributor or reference site; read 2026-11-17)
- Aircraft Materials (UK stockist): Stainless Steel 17-4PH Bar (AMS 5643 / AMS 5622) Technical Data Sheet aircraftmaterials.com/data/alstst/ams5643.html (distributor or reference site; read 2026-11-17)
Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.