303 stainless steel (EN 1.4305)

Properties of 303 stainless steel (EN 1.4305), each value tied to a recorded source.

The free-machining stainless steel. Added sulfur makes it the easiest stainless to turn and mill, so it is the usual choice for screw-machine parts such as shafts, fittings and fasteners. The trade-off is lower corrosion resistance than 304, poor weldability and less formability.

Family
Stainless steels: austenitic
Condition
Annealed (solution treated); data for bar up to 160 mm
Common forms
Round and hex bar, wire
EN
1.4305
Common name
303
UNS
S30300 (per Aalco, not a direct equivalent)
Relative cost
$$ Editorial, relative: a little above 304 as bar, and cheaper to machine. Not a quote; prices change.

Composition

Weight percent. The sources agree on every limit except the sulfur maximum (0.35 and 0.15 percent), so sulfur and the extra elements come from Aalco only.

ElementLimitsSource
Carbon (C)0.10 max1,2
Chromium (Cr)17.00 to 19.001,2
Manganese (Mn)2.00 max1,2
Silicon (Si)1.00 max1,2
Nickel (Ni)8.00 to 10.001,2
Sulfur (S)0.15 to 0.351
Phosphorus (P)0.05 max1
Iron (Fe)balance1,2

Properties

PropertySIUS customaryBasisSource
Physical
Density8.030 g/cm³0.290 lb/in³typical1
Density8.030 g/cm³0.290 lb/in³typical, printed as 8.03 kg/m³, a units slip for g/cm³2
Mechanical
Elastic modulus (Young's)193.0 GPa28.0 Msitypical1
Elastic modulus (Young's)193.0 GPa28.0 Msitypical2
Yield strength190 MPa27.6 ksiminimum, proof stress, bar up to 160 mm1
Yield strength190 MPa27.6 ksiminimum, proof stress, minimum2
Tensile strength (ultimate or at break)500 to 750 MPa72.5 to 109 ksirange, bar up to 160 mm1
Tensile strength (ultimate or at break)500 to 700 MPa72.5 to 102 ksirange2
Elongation at break35 %minimum, A50 mm, bar up to 160 mm1
Elongation at break35 %typical, A52
Hardness, Brinell (HB)230 HBmaximum, Brinell, bar up to 160 mm1
Thermal
Melting point (as published)1,455 °C2,651 °Ftypical, published as a single melting point1
Melting point (as published)1,455 °C2,651 °Ftypical, published as a single melting point2
Thermal conductivity16 W/m·K113 BTU·in/h·ft²·°Ftypical, temperature not stated1
Thermal conductivity16 W/m·K113 BTU·in/h·ft²·°Ftypical, temperature not stated2
Thermal expansion (linear)17.3 µm/m·K9.61 µin/in·°Ftypical, temperature range not stated1
Thermal expansion (linear)17.3 µm/m·K9.61 µin/in·°Ftypical, temperature range not stated2
Electrical
Electrical resistivity720 nΩ·mtypical, printed as 0.72 x10^-6 ohm·m1

What the sources say

  • Aalco calls 303 the most readily machinable austenitic stainless steel, says its sulfur lowers corrosion resistance and gives poor weldability, and says it is not suitable for marine environments. 1
  • Smiths Metal Centres rates 303 machinability as very good, weldability as poor and corrosion resistance as good in mild environments, and says it is not recommended for any application involving welding. 2

Things to know

  • Two distributor sources; both call their data indicative, so confirm against the standard and your material certificate.
  • The tensile ranges differ slightly (500 to 750 and 500 to 700 MPa); the range is shown.

Sources

  1. Aalco Metals Limited: Stainless Steel, Austenitic, 1.4305 (303) Bar (data per EN 10088-3:2005) aalco.co.uk/datasheets/Stainless-Steel-14305-303-Bar_107.ashx (distributor or reference site; read 2026-11-17)
  2. Smiths Metal Centres: 303 Stainless Technical Datasheet smithmetal.com/pdf/stainless/303-stainless.pdf (distributor or reference site; read 2026-11-17)

Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.