304 stainless steel (EN 1.4301)
Properties of 304 stainless steel (EN 1.4301), each value tied to a recorded source.
The standard general-purpose stainless steel: good corrosion resistance, easy to form and weld, and not hardenable by heat treatment. It is the usual choice for food equipment, enclosures and fasteners, and it work-hardens quickly when machined.
Composition
Weight percent, per EN 10088-3:2005 as listed by the source.
| Element | Limits | Source |
|---|---|---|
| Carbon (C) | 0.07 max | 1,2 |
| Chromium (Cr) | 17.50 to 19.50 | 1,2 |
| Manganese (Mn) | 2.00 max | 1,2 |
| Silicon (Si) | 1.00 max | 1,2 |
| Phosphorus (P) | 0.05 max | 1,2 |
| Sulfur (S) | 0.03 max | 1 |
| Nickel (Ni) | 8.00 to 10.50 | 1,2 |
| Nitrogen (N) | 0.11 max | 1 |
| Iron (Fe) | balance | 1,2 |
Properties
| Property | SI | US customary | Basis | Source |
|---|---|---|---|---|
| Physical | ||||
| Density | 8.000 g/cm³ | 0.289 lb/in³ | typical, typical for bar and section | 1 |
| Density | 8.000 g/cm³ | 0.289 lb/in³ | typical, printed as 8.00 kg/m³, a units slip for about 8000 kg/m³ | 2 |
| Mechanical | ||||
| Elastic modulus (Young's) | 193.0 GPa | 28.0 Msi | typical | 1 |
| Elastic modulus (Young's) | 193.0 GPa | 28.0 Msi | typical | 2 |
| Yield strength | 190 MPa | 27.6 ksi | minimum, proof stress, bar and section up to 160 mm (the source does not name the offset) | 1 |
| Yield strength | 210 MPa | 30.5 ksi | minimum, proof stress, minimum | 2 |
| Tensile strength (ultimate or at break) | 500 to 700 MPa | 72.5 to 102 ksi | range, bar and section up to 160 mm | 1 |
| Tensile strength (ultimate or at break) | 500 to 700 MPa | 72.5 to 102 ksi | range | 2 |
| Elongation at break | 45 % | minimum, A50 mm, bar and section up to 160 mm | 1 | |
| Elongation at break | 45 % | minimum, A5, minimum | 2 | |
| Hardness, Brinell (HB) | 215 HB | maximum, Brinell, bar and section up to 160 mm | 1 | |
| Thermal | ||||
| Melting point (as published) | 1,450 °C | 2,642 °F | typical, published as a single melting point | 2 |
| Thermal conductivity | 16 W/m·K | 112 BTU·in/h·ft²·°F | typical, temperature not stated | 1 |
| Thermal conductivity | 16 W/m·K | 112 BTU·in/h·ft²·°F | typical, temperature not stated | 2 |
| Thermal expansion (linear) | 17.2 µm/m·K | 9.56 µin/in·°F | typical, temperature range not stated | 1 |
| Thermal expansion (linear) | 17.2 µm/m·K | 9.56 µin/in·°F | typical, temperature range not stated | 2 |
| Electrical | ||||
| Electrical resistivity | 720 nΩ·m | typical, printed as 0.72 x10^-6 ohm·m | 1 | |
What the sources say
- The source says 304 can pit and crevice-corrode in chloride environments and can suffer stress corrosion cracking above 60 °C. 1
- The source says 304 cannot be hardened by heat treatment, and gives 1010 to 1120 °C for solution treatment or annealing. 1
- The source rates fusion welding of 304 as excellent and recommends grade 308 filler (308L for 304L). 1
Things to know
- Two distributor sources (Aalco, per EN 10088-3, and Smiths, a 304 and 304L sheet); both call their data indicative, so confirm against the standard and your material certificate.
- The sources differ slightly on minimum proof stress (190 and 210 MPa) and on the sulfur limit (0.03 and 0.02 percent); the range is shown. Smiths prints density as 8.00 kg/m³, a units slip for 8.00 g/cm³.
Sources
- Aalco Metals Limited: Stainless Steel, Austenitic, 1.4301 (304) Bar and Section (data per EN 10088-3:2005) aalco.co.uk/datasheets/Stainless-Steel-14301-Bar-and-Section_34.ashx (distributor or reference site; read 2026-11-17)
- Smiths Metal Centres: 304 / 304L Stainless Technical Datasheet smithmetal.com/pdf/stainless/304-304l-stainless.pdf (distributor or reference site; read 2026-11-17)
Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.