316 stainless steel (EN 1.4401)
Properties of 316 stainless steel (EN 1.4401), each value tied to a recorded source.
Stainless steel with molybdenum added for better resistance to chlorides and pitting than 304. It is the usual choice near salt water and in chemical and food processing, and it costs more than 304.
Composition
Weight percent per EN 10088-3:2005 as listed by the source.
| Element | Limits | Source |
|---|---|---|
| Carbon (C) | 0.07 max | 1 |
| Chromium (Cr) | 16.50 to 18.50 | 1,2 |
| Molybdenum (Mo) | 2.00 to 2.50 | 1,2 |
| Silicon (Si) | 1.00 max | 1,2 |
| Phosphorus (P) | 0.05 max | 1,2 |
| Sulfur (S) | 0.03 max | 1 |
| Nickel (Ni) | 10.00 to 13.00 | 1,2 |
| Manganese (Mn) | 2.00 max | 1,2 |
| Nitrogen (N) | 0.11 max | 1 |
| Iron (Fe) | balance | 1,2 |
Properties
| Property | SI | US customary | Basis | Source |
|---|---|---|---|---|
| Physical | ||||
| Density | 8.000 g/cm³ | 0.289 lb/in³ | typical, typical for bar and section | 1 |
| Density | 8.000 g/cm³ | 0.289 lb/in³ | typical, printed as 8.00 kg/m³, a units slip for about 8000 kg/m³ | 2 |
| Mechanical | ||||
| Elastic modulus (Young's) | 193.0 GPa | 28.0 Msi | typical | 1 |
| Elastic modulus (Young's) | 193.0 GPa | 28.0 Msi | typical | 2 |
| Yield strength | 200 MPa | 29.0 ksi | minimum, proof stress, bar and section up to 160 mm | 1 |
| Yield strength | 220 MPa | 31.9 ksi | minimum, proof stress, minimum | 2 |
| Tensile strength (ultimate or at break) | 500 to 700 MPa | 72.5 to 102 ksi | range, bar and section up to 160 mm | 1 |
| Tensile strength (ultimate or at break) | 520 to 680 MPa | 75.4 to 98.6 ksi | range | 2 |
| Elongation at break | 40 % | minimum, A50 mm, bar and section up to 160 mm | 1 | |
| Elongation at break | 40 % | minimum, A5, minimum | 2 | |
| Hardness, Brinell (HB) | 215 HB | maximum, Brinell, bar and section up to 160 mm | 1 | |
| Thermal | ||||
| Melting point (as published) | 1,400 °C | 2,552 °F | typical, published as a single melting point | 1 |
| Melting point (as published) | 1,400 °C | 2,552 °F | typical, published as a single melting point | 2 |
| Thermal conductivity | 16 W/m·K | 113 BTU·in/h·ft²·°F | typical, temperature not stated | 1 |
| Thermal conductivity | 16 W/m·K | 113 BTU·in/h·ft²·°F | typical, temperature not stated | 2 |
| Thermal expansion (linear) | 15.9 µm/m·K | 8.83 µin/in·°F | typical, temperature range not stated | 1 |
| Thermal expansion (linear) | 15.9 µm/m·K | 8.83 µin/in·°F | typical, temperature range not stated | 2 |
| Electrical | ||||
| Electrical resistivity | 740 nΩ·m | typical, printed as 0.74 x10^-6 ohm·m | 1 | |
What the sources say
- The source describes 316 as usually regarded as marine grade stainless steel but not resistant to warm sea water, with pitting and crevice corrosion possible in warm chloride environments and stress corrosion cracking above about 60 °C. 1
Things to know
- Two distributor sources (Aalco, per EN 10088-3, and Smiths, a 316 and 316L sheet); both call their data indicative, so confirm against the standard and your material certificate.
- The sources differ on minimum proof stress (200 and 220 MPa), the carbon limit (0.07 and 0.08 percent) and the sulfur limit; the range is shown. Smiths prints density as 8.00 kg/m³, a units slip for 8.00 g/cm³.
Sources
- Aalco Metals Limited: Stainless Steel, Austenitic, 1.4401 (316) Bar and Section (data per EN 10088-3:2005) aalco.co.uk/datasheets/Stainless-Steel-14401-316-Bar-and-Section_37.ashx (distributor or reference site; read 2026-11-17)
- Smiths Metal Centres: 316 / 316L Stainless Technical Datasheet smithmetal.com/pdf/stainless/316-316l-stainless.pdf (distributor or reference site; read 2026-11-17)
Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.