321 stainless steel (UNS S32100)
Properties of 321 stainless steel (UNS S32100), each value tied to a recorded source.
A version of 304 stainless steel with titanium added as a stabilizer. The titanium reduces carbide precipitation during welding, so the grade resists intergranular corrosion after welding and after long periods at elevated temperature. It is used for exhausts, manifolds, heat exchangers and refinery equipment.
Composition
Weight percent. All three sources agree on carbon, manganese, sulfur, chromium, nickel and nitrogen. Phosphorus is 0.04 in Aalco and Aircraft Materials but 0.045 in Smiths, so Smiths is not cited for it. Silicon is 0.75 max in Smiths and Aalco but 0.25 to 1.00 in Aircraft Materials (AMS 5510), so Aircraft Materials is not cited for it. Titanium: Smiths gives a minimum of 5 x (C + N) and 0.70 max, Aircraft Materials 0.7 max; Aalco prints 0.07 max, which looks like a slip, so Aalco is not cited for titanium. Copper and molybdenum limits come from Aircraft Materials (AMS 5510) only.
| Element | Limits | Source |
|---|---|---|
| Carbon (C) | 0.08 max | 3,1,2 |
| Manganese (Mn) | 2.00 max | 3,1,2 |
| Sulfur (S) | 0.03 max | 3,1,2 |
| Chromium (Cr) | 17.00 to 19.00 | 3,1,2 |
| Nickel (Ni) | 9.00 to 12.00 | 3,1,2 |
| Nitrogen (N) | 0.10 max | 3,1,2 |
| Phosphorus (P) | 0.04 max | 3,2 |
| Silicon (Si) | 0.75 max | 1,2 |
| Titanium (Ti) | 0.70 max | 1,3 |
| Copper (Cu) | 0.75 max | 3 |
| Molybdenum (Mo) | 0.75 max | 3 |
| Iron (Fe) | balance | 3,2 |
Properties
| Property | SI | US customary | Basis | Source |
|---|---|---|---|---|
| Mechanical | ||||
| Elastic modulus (Young's) | 193.0 GPa | 28.0 Msi | typical | 1 |
| Yield strength | 205 MPa | 29.7 ksi | typical, proof stress; printed without a stated basis | 1 |
| Yield strength | 205 MPa | 29.7 ksi | minimum, proof stress, sheet to ASTM A240 | 2 |
| Yield strength | 172 MPa | 25.0 ksi | typical, AMS 5510 sheet, solution treated (25 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 3 |
| Tensile strength (ultimate or at break) | 515 MPa | 74.7 ksi | minimum | 1 |
| Tensile strength (ultimate or at break) | 515 MPa | 74.7 ksi | minimum, sheet to ASTM A240 | 2 |
| Tensile strength (ultimate or at break) | 483 to 690 MPa | 70.0 to 100 ksi | range, AMS 5510 sheet, solution treated (70 to 100 ksi) (Printed in ksi; converted at 1 ksi = 6.894757 MPa and rounded to 0.1 MPa.) | 3 |
| Elongation at break | 40 % | typical, A5; printed without a stated basis | 1 | |
| Elongation at break | 35 % | minimum, A50 mm, sheet to ASTM A240 | 2 | |
| Elongation at break | 40 % | typical, AMS 5510 sheet, solution treated | 3 | |
| Hardness, Brinell (HB) | 255 HB | maximum, AMS 5645 bar, solution treated | 3 | |
| Thermal | ||||
| Melting point (as published) | 1,400 °C | 2,552 °F | typical, published as a single melting point | 1 |
| Thermal conductivity | 16 W/m·K | 112 BTU·in/h·ft²·°F | typical, at 100 °C | 1 |
Specifications
- AMS 5510: sheet, strip and plate 3
- AMS 5645: bars, wire and forgings 3
- ASTM A240: sheet (composition and mechanical minimums as cited by Aalco) 2
What the sources say
- Smiths Metal Centres says the titanium content is typically five times the carbon content, which reduces carbide precipitation during welding and improves elevated-temperature properties, and that 321 is more difficult to form than other austenitic grades but weldable by common fusion and resistance methods. 1
- Aircraft Materials says 321 is used where resistance to intergranular corrosion is needed and parts are held for long periods at 800 to 1500 °F, for example exhaust stacks, manifolds and ring collectors. 3
Things to know
- Three distributor sources; all disclaim their data (indicative, approximate or guideline only), so confirm against the specification and your material certificate.
- No density is given: Smiths prints it as 8.09 g/m³, a units slip, and the other two sources do not give one. Smiths also prints electrical resistivity as 0.074 x10^-6 ohm·m, which looks off by ten, so it is not used either.
- Tensile strength: Smiths and Aalco give 515 MPa minimum; Aircraft Materials gives 70 to 100 ksi (about 483 to 690 MPa) as typical for AMS 5510 sheet. Proof stress is 205 MPa (Aalco minimum, Smiths without a basis) against 25 ksi (about 172 MPa) in Aircraft Materials. All are shown.
Sources
- Smiths Metal Centres: 321 Stainless Technical Datasheet smithmetal.com/pdf/stainless/321-stainless.pdf (distributor or reference site; read 2026-11-17)
- Aalco Metals Limited: Stainless Steel, S32100 (321) Sheet (data per ASTM A240) aalco.co.uk/datasheets/Stainless-Steel-S32100-Sheet_268.ashx (distributor or reference site; read 2026-11-17)
- Aircraft Materials (UK stockist): Stainless Steel 321 (AMS 5510 / AMS 5645) Technical Data Sheet aircraftmaterials.com/data/alstst/ams5510.html (distributor or reference site; read 2026-11-17)
Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.