410 stainless steel (EN 1.4006)

Properties of 410 stainless steel (EN 1.4006), each value tied to a recorded source.

The common hardenable stainless steel. It is magnetic, can be heat treated to high hardness and is used for valve parts, pump shafts, fasteners and cutlery. Its corrosion resistance is moderate (below 304) and it is hard to weld.

Family
Stainless steels: martensitic
Condition
Data for bar up to 160 mm in the supplied (hardened and tempered or annealed) condition; strength depends on heat treatment
Common forms
Round bar, plate and sheet
EN
1.4006
Common name
410
UNS
S41000 (per Aalco, not a direct equivalent)
Relative cost
$$ Editorial, relative: similar to 304 stainless steel as bar. Not a quote; prices change.

Composition

Weight percent. The sources agree on carbon (to 0.15), chromium, silicon, phosphorus and nickel; manganese and sulfur limits differ, so those come from Aalco only.

ElementLimitsSource
Carbon (C)0.15 max1,2
Chromium (Cr)11.50 to 13.501,2
Silicon (Si)1.00 max1,2
Phosphorus (P)0.04 max1,2
Nickel (Ni)0.75 max1,2
Manganese (Mn)1.50 max1
Sulfur (S)0.02 max1
Iron (Fe)balance1,2

Properties

PropertySIUS customaryBasisSource
Physical
Density7.750 g/cm³0.280 lb/in³typical1
Density7.800 g/cm³0.282 lb/in³typical, printed as 7800 kg/m³2
Mechanical
Elastic modulus (Young's)200.0 GPa29.0 Msitypical2
Yield strength450 MPa65.3 ksiminimum, proof stress, bar up to 160 mm1
Yield strength495 MPa71.8 ksitypical, yield strength2
Tensile strength (ultimate or at break)650 to 850 MPa94.3 to 123 ksirange, bar up to 160 mm1
Tensile strength (ultimate or at break)700 to 850 MPa102 to 123 ksirange2
Elongation at break15 %minimum, A, bar up to 160 mm1
Elongation at break15 %typical, A52
Thermal
Melting point (as published)1,400 °C2,552 °Ftypical, published as a single melting point2
Thermal conductivity25 W/m·K173 BTU·in/h·ft²·°Ftypical, temperature not stated1
Thermal conductivity25 W/m·K173 BTU·in/h·ft²·°Ftypical, at 100 °C2
Thermal expansion (linear)9.9 µm/m·K5.50 µin/in·°Ftypical, temperature range not stated1
Electrical
Electrical resistivity570 nΩ·mtypical, printed as 0.57 x10^-6 ohm·m1
Electrical resistivity570 nΩ·mtypical, printed as 570 nΩ·m2

What the sources say

  • Smiths Metal Centres calls 410 a commonly used martensitic stainless steel with excellent hardness after heat treatment, limited corrosion resistance and poor weldability, and says machining gets difficult above 30 HRC. 2
  • Aalco describes the corrosion resistance of 1.4006 as moderate in environments without chlorides. 1

Things to know

  • Two distributor sources; both call their data indicative, so confirm against the standard and your material certificate. Strength depends strongly on heat treatment.
  • Aalco prints the elastic modulus as 300 GPa, which looks like a typo (Smiths gives 200 GPa); only the Smiths value is recorded.

Sources

  1. Aalco Metals Limited: Stainless Steel, 1.4006 (410) Bar (data per EN 10088-3:2005) aalco.co.uk/datasheets/Stainless-Steel-14006-Bar_315.ashx (distributor or reference site; read 2026-11-17)
  2. Smiths Metal Centres: 410 Stainless Technical Datasheet smithmetal.com/pdf/stainless/410-stainless.pdf (distributor or reference site; read 2026-11-17)

Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.

All materials

Published by Nick Peterson, mechanical engineer.