416 stainless steel (EN 1.4005)
Properties of 416 stainless steel (EN 1.4005), each value tied to a recorded source.
The free-machining version of 410: sulfur makes it easy to turn and mill, and it can be hardened. It is used for shafts, gears, bolts, nuts and screw-machine parts. Its corrosion resistance is lower than 304 and it is unsuitable for marine or chloride exposure.
Composition
Weight percent. The sources agree on chromium, manganese, silicon, phosphorus and sulfur; the carbon lower limit differs (0.06 and 0.08), so carbon comes from Aalco only.
| Element | Limits | Source |
|---|---|---|
| Chromium (Cr) | 12.00 to 14.00 | 1,2 |
| Manganese (Mn) | 1.50 max | 1,2 |
| Silicon (Si) | 1.00 max | 1,2 |
| Phosphorus (P) | 0.04 max | 1,2 |
| Sulfur (S) | 0.15 to 0.35 | 1,2 |
| Carbon (C) | 0.06 to 0.15 | 1 |
| Molybdenum (Mo) | 0.60 max | 1 |
| Iron (Fe) | balance | 1,2 |
Properties
| Property | SI | US customary | Basis | Source |
|---|---|---|---|---|
| Physical | ||||
| Density | 7.750 g/cm³ | 0.280 lb/in³ | typical | 1 |
| Density | 7.750 g/cm³ | 0.280 lb/in³ | typical, printed as 7.75 g/cm³ | 2 |
| Mechanical | ||||
| Elastic modulus (Young's) | 200.0 GPa | 29.0 Msi | typical | 1 |
| Elastic modulus (Young's) | 200.0 GPa | 29.0 Msi | typical | 2 |
| Yield strength | 450 MPa | 65.3 ksi | minimum, proof stress, bar up to 160 mm | 1 |
| Yield strength | 280 to 1,110 MPa | 40.6 to 161 ksi | range, proof stress across heat treatments | 2 |
| Tensile strength (ultimate or at break) | 650 to 850 MPa | 94.3 to 123 ksi | range, bar up to 160 mm | 1 |
| Tensile strength (ultimate or at break) | 500 to 1,400 MPa | 72.5 to 203 ksi | range, across heat treatments | 2 |
| Elongation at break | 11 to 30 % | range, A5 across heat treatments | 2 | |
| Thermal | ||||
| Thermal conductivity | 25 W/m·K | 173 BTU·in/h·ft²·°F | typical, temperature not stated | 1 |
| Thermal conductivity | 25 W/m·K | 173 BTU·in/h·ft²·°F | typical, temperature not stated | 2 |
| Thermal expansion (linear) | 9.9 µm/m·K | 5.50 µin/in·°F | typical, temperature range not stated | 1 |
| Thermal expansion (linear) | 9.9 µm/m·K | 5.50 µin/in·°F | typical, temperature range not stated | 2 |
| Electrical | ||||
| Electrical resistivity | 570 nΩ·m | typical, printed as 0.57 x10^-6 ohm·m | 1 | |
What the sources say
- Aalco says 416 is totally unsuitable for marine or other chloride exposure, with corrosion resistance lower than the common austenitic grades, and lists valve parts, pump and motor shafts, gears, bolts and automatic screw-machined parts as typical uses. 1
- Smiths Metal Centres says the mechanical properties of 416 vary greatly with the heat treatment the material has had. 2
Things to know
- Two distributor sources; both call their data indicative, so confirm against the standard and your material certificate. The two strength entries are on different bases (a bar specification and a range across heat treatments).
- Smiths prints electrical resistivity as 0.057 x10^-6, which looks off by ten, so it is not used.
Sources
- Aalco Metals Limited: Stainless Steel, 1.4005 (416) Bar (data per EN 10088-3:2005) aalco.co.uk/datasheets/Stainless-Steel-14005-416-Bar_108.ashx (distributor or reference site; read 2026-11-17)
- Smiths Metal Centres: 416 Stainless Technical Datasheet smithmetal.com/pdf/stainless/416-stainless.pdf (distributor or reference site; read 2026-11-17)
Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.