430 stainless steel (EN 1.4016)
Properties of 430 stainless steel (EN 1.4016), each value tied to a recorded source.
The common low-cost ferritic stainless steel. It is magnetic, holds up well in mild environments and forms and welds acceptably, so it is used for sinks, appliances and trim. It has lower corrosion resistance than 304, no nickel, and cannot be hardened by heat treatment.
Composition
Weight percent. The sources agree on carbon, chromium, manganese, silicon and phosphorus; the sulfur limit differs (0.03 and 0.02), so sulfur comes from Aalco only.
| Element | Limits | Source |
|---|---|---|
| Carbon (C) | 0.08 max | 1,2 |
| Chromium (Cr) | 16.00 to 18.00 | 1,2 |
| Manganese (Mn) | 1.00 max | 1,2 |
| Silicon (Si) | 1.00 max | 1,2 |
| Phosphorus (P) | 0.04 max | 1,2 |
| Sulfur (S) | 0.03 max | 1 |
| Iron (Fe) | balance | 1,2 |
Properties
| Property | SI | US customary | Basis | Source |
|---|---|---|---|---|
| Physical | ||||
| Density | 7.750 g/cm³ | 0.280 lb/in³ | typical | 1 |
| Density | 7.750 g/cm³ | 0.280 lb/in³ | typical, printed as 7.75 g/cm³ | 2 |
| Mechanical | ||||
| Elastic modulus (Young's) | 200.0 GPa | 29.0 Msi | typical | 1 |
| Elastic modulus (Young's) | 200.0 GPa | 29.0 Msi | typical | 2 |
| Yield strength | 240 MPa | 34.8 ksi | minimum, proof stress, bar up to 100 mm | 1 |
| Yield strength | 240 MPa | 34.8 ksi | minimum, proof stress, minimum | 2 |
| Tensile strength (ultimate or at break) | 400 to 630 MPa | 58.0 to 91.4 ksi | range, bar up to 100 mm | 1 |
| Tensile strength (ultimate or at break) | 450 to 600 MPa | 65.3 to 87.0 ksi | range | 2 |
| Elongation at break | 20 % | minimum, A50 mm, bar up to 100 mm | 1 | |
| Elongation at break | 20 % | typical, A5 | 2 | |
| Hardness, Brinell (HB) | 200 HB | maximum, Brinell, bar up to 100 mm | 1 | |
| Thermal | ||||
| Melting point (as published) | 1,425 to 1,510 °C | 2,597 to 2,750 °F | range, melting range | 1 |
| Melting point (as published) | 1,425 to 1,510 °C | 2,597 to 2,750 °F | range, melting range | 2 |
| Thermal conductivity | 24 W/m·K | 166 BTU·in/h·ft²·°F | typical, temperature not stated | 1 |
| Thermal conductivity | 24 W/m·K | 166 BTU·in/h·ft²·°F | typical, temperature not stated | 2 |
| Thermal expansion (linear) | 10.4 µm/m·K | 5.78 µin/in·°F | typical, temperature range not stated | 1 |
| Thermal expansion (linear) | 10.4 µm/m·K | 5.78 µin/in·°F | typical, temperature range not stated | 2 |
| Electrical | ||||
| Electrical resistivity | 600 nΩ·m | typical, printed as 0.60 x10^-6 ohm·m | 1 | |
What the sources say
- Smiths Metal Centres rates the corrosion resistance of 430 as good but below the austenitic grades, says it forms well, welds readily but is not suited to rigorous service, and notes a risk of galling when machined. 2
Things to know
- Two distributor sources; both call their data indicative, so confirm against the standard and your material certificate. The tensile ranges differ slightly (400 to 630 and 450 to 600 MPa); the range is shown.
- Smiths prints electrical resistivity as 0.060 x10^-6, which looks off by ten, so it is not used.
Sources
- Aalco Metals Limited: Stainless Steel, 1.4016 (430) Bar (data per EN 10088-3:2005) aalco.co.uk/datasheets/Stainless-Steel-14016-430-Bar_348.ashx (distributor or reference site; read 2026-11-17)
- Smiths Metal Centres: 430 Stainless Technical Datasheet smithmetal.com/pdf/stainless/430-stainless.pdf (distributor or reference site; read 2026-11-17)
Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.