Ti-6Al-4V (grade 5) titanium
Properties of Ti-6Al-4V (grade 5) titanium, each value tied to a recorded source.
The most widely used titanium alloy. It is about 60 percent as dense as steel with strength like a good alloy steel and excellent corrosion resistance, but it is expensive, hard to machine and weld, and loses strength above about 400 °C. It is used in aerospace, medical implants, racing and marine parts.
Composition
Weight percent. Aircraft Materials prints its iron limit as 0.03, which looks like a typo (0.30 or 0.40); the Smiths value is used.
| Element | Limits | Source |
|---|---|---|
| Aluminum (Al) | 5.50 to 6.75 | 2,1 |
| Vanadium (V) | 3.50 to 4.50 | 2,1 |
| Carbon (C) | 0.08 max | 2,1 |
| Nitrogen (N) | 0.05 max | 2,1 |
| Oxygen (O) | 0.20 max | 2,1 |
| Hydrogen (H) | 0.02 max | 2,1 |
| Iron (Fe) | 0.40 max | 1 |
| Titanium (Ti) | balance | 2,1 |
Properties
| Property | SI | US customary | Basis | Source |
|---|---|---|---|---|
| Physical | ||||
| Density | 4.420 g/cm³ | 0.160 lb/in³ | typical, printed as 4.42 kg/dm³ | 1 |
| Mechanical | ||||
| Elastic modulus (Young's) | 114.0 GPa | 16.5 Msi | typical, elastic modulus | 1 |
| Yield strength | 828 MPa | 120 ksi | minimum, 0.2 % proof stress, bar to ASTM B348 grade 5 | 1 |
| Yield strength | 910 MPa | 132 ksi | typical, 0.2 % proof stress, bar to ASTM B348 grade 5 | 1 |
| Yield strength | 862 MPa | 125 ksi | minimum, annealed bar under 2.00 in (125 ksi) | 2 |
| Yield strength | 827 MPa | 120 ksi | minimum, annealed bar 2.00 to 4.00 in and over 4.00 in (120 ksi) | 2 |
| Tensile strength (ultimate or at break) | 895 MPa | 130 ksi | minimum, bar to ASTM B348 grade 5 | 1 |
| Tensile strength (ultimate or at break) | 1,000 MPa | 145 ksi | typical, bar to ASTM B348 grade 5 | 1 |
| Tensile strength (ultimate or at break) | 931 MPa | 135 ksi | minimum, annealed bar under 2.00 in (135 ksi) | 2 |
| Tensile strength (ultimate or at break) | 896 MPa | 130 ksi | minimum, annealed bar 2.00 in and over (130 ksi) | 2 |
| Elongation at break | 10 % | minimum, in 4 diameters, bar to ASTM B348 grade 5 | 1 | |
| Elongation at break | 18 % | typical, in 4 diameters, bar to ASTM B348 grade 5 | 1 | |
| Elongation at break | 10 % | minimum, in 2 in, annealed bar up to 4 in; 8 % over 4 in | 2 | |
Specifications
- ASTM B348 Grade 5: titanium and titanium alloy bars and billets 1
- AMS 4928: Ti-6Al-4V bar, wire, forgings and rings, annealed 2
What the sources say
- Smiths Metal Centres calls grade 5 the most widely used high-strength titanium alloy, rates its weldability as fair, and says it can be used up to around 400 °C. 1
Things to know
- The sources are on different bases: Smiths gives both a minimum and a typical value; Aircraft Materials gives annealed-bar minimums by diameter. Heat-treated and larger sections differ. None is a design value.
- Grade 23 (ELI) has lower oxygen, better ductility and fracture toughness and somewhat lower strength; it is a different material.
Sources
- Smiths Metal Centres: Ti-6Al-4V (Grade 5) Technical Datasheet smithmetal.com/pdf/titanium/ti-6al-4v-grade-5.pdf (distributor or reference site; read 2026-11-17)
- Aircraft Materials (UK stockist): Titanium Alloy Grade 5 / Ti-6Al-4V Technical Data Sheet aircraftmaterials.com/data/titanium/ti6al4v.html (distributor or reference site; read 2026-11-17)
Typical values are not guaranteed and must not be used as design minimums. Minimum and maximum values apply to the forms, thicknesses and conditions stated. Where two sources differ, both are shown. Always confirm with the specification, the material certificate and your supplier before you rely on a number. The values were read from the cited sources on 2026-11-17.